Composite machining technical article | Nabak Composite

Cutting and Machining Composite Parts: From Cutting and Drilling to Bonding and Painting — A Practical Engineering Guide

In this article we look at all the workshop operations on composite parts from an engineering point of view: why machining composites differs from metal, choosing tools and speeds for cutting composites, drilling, milling, turning, punching and sanding, joining with bolts and rivets, bonding with epoxy and polyurethane, and painting composite surfaces for outdoor use.

Publisher: Nabak Composite Topic: Machining and installing composites Reading time: about 25 minutes

Why is machining composite parts different from metals?

Workshop tools for working with composite parts look somewhat like woodworking and aluminum tools, and composite profiles, sheets and tubes can be cut, drilled, milled, punched and sanded. But the material behaves completely differently under the tool, and ignoring these differences leads to poor edge quality, damaged parts and rapid tool wear. Four main characteristics set machining composites apart from metals:

  • Abrasive glass fibers: glass fiber is nearly as hard as many tool steels, so ordinary high-speed steel (HSS) tools blunt quickly and tungsten carbide or diamond tools must be used.
  • Anisotropy and layered structure: at every moment the tool meets fibers and resin with very different properties. At the tool's exit edge, plies may separate (delamination) or the fibers may fray.
  • Low thermal conductivity: heat stays at the cutting zone, and with the wrong speed or pressure the resin at the cut edge softens or burns.
  • Dust instead of chips: machining composites produces fine fiber and resin dust instead of continuous chips, which requires extraction and respiratory protection.
Safety note: because glass fiber and polyester resin dust is produced during cutting, drilling and sanding, always wear a respirator, safety glasses and gloves, and work in a well-ventilated area or preferably outdoors. Full details are in safety with composite products.
Cutting a composite box section with a diamond blade in the Nabak Composite workshop
Cutting a composite with a diamond circular saw in the Nabak workshop: holding the part without vibration and feeding slowly and evenly is the key to a clean cut.

Choosing the tool material for machining composites

Tool materialTool life in compositesEdge qualityRecommended application
High-speed steel (HSS)Very shortPoor once bluntOnly very limited, temporary work
Tungsten carbideGoodGoodDrills, toothed saw blades, milling and turning tools
Diamond (electroplated or set diamond grit)Very goodVery goodDiamond cutting discs, hole saws and diamond drills
Polycrystalline diamond (PCD)ExcellentExcellentMass production and CNC machining
Aluminum oxide abrasive discModerateMedium, with a lot of heatLimited workshop cuts; not recommended for high quality

Cutting polymer-matrix composites

Cutting is the most common workshop operation on composite profiles, sheets and tubes. The cutting method is chosen according to the volume of work, part thickness and required accuracy:

  • Hand hacksaw: for small amounts of cutting and on site, a hacksaw with a fine-tooth blade (24 to 32 teeth per inch) or a carbide-grit blade can be used.
  • Circular saw with a diamond or carbide blade: the standard method for cutting composites in the workshop and factory. The blade diameter is 200 to 500 mm depending on the thickness of the composite part.
  • Jigsaw with a carbide-grit blade: for curved and window cut-outs in composite sheet.
  • Band saw with a carbide-grit or diamond blade: for cutting thick sections and long cuts.
  • Abrasive waterjet: precise cutting with no heat and little dust; suitable for complex shapes in composite sheet.
  • CNC router: for mass-producing precisely shaped parts from sheet and panels.
Laser cutting is not recommended: a laser burns the resin, leaves a charred, weak edge and produces toxic fumes. Grinding the surface of parts with an angle grinder and grinding disc is also prohibited (see the sanding section).
Cutting a composite with a diamond disc and water coolant
Cutting a composite with a diamond disc and water as coolant; the cut edge quality after fine sanding.
Cutting a fiberglass profile with a profile saw in a composite workshop
Cutting a fiberglass profile with a profile saw; the clamp holds the part firmly without vibration.

Cutting speed and calculating blade rpm

The suitable peripheral speed for cutting composites with a diamond or carbide blade is about 1800 to 3600 m/min. The required motor speed is calculated from the following formula:

n (rpm) = vc (m/min) / ( π × D (m) )
Blade diameter (mm)rpm for 1800 m/minrpm for 3600 m/min
200approx. 2900approx. 5700
300approx. 1900approx. 3800
400approx. 1400approx. 2900
500approx. 1150approx. 2300

Note that the maximum permitted speed marked on the blade must never be exceeded.

Instructions for a quality cut

  1. Marking: draw the cut line on paper masking tape to reduce edge chipping
  2. Fixing: clamp the part firmly, with no vibration
  3. Feed: cut slowly with low, even force
  4. Cooling: use water or coolant to reduce heat and dust
  5. Finishing: clean up the cut with fine sandpaper
  6. Sealing: coat the cut edge with a thin layer of resin

Common defects in cutting composites and how to fix them

DefectCauseSolution
Fiber fraying at the edgeBlunt tool, coarse teeth, fast feedReplace or sharpen the tool, use a diamond blade, slow the feed
Chipping and delamination at the cut exitNo support at the end of the cutWooden support or a sacrificial piece under and behind the part
Burning and discoloration of the edgeToo much heat, wrong speed, blunt bladeCoolant, less pressure, sharp blade
Crooked, out-of-square cutPart vibration or blade wobbleClamp the part and check the blade

Drilling composites

Drilling is the most common operation after cutting and a prerequisite for almost all mechanical connections. The right drill for composite parts depends on the hole diameter:

  • Holes up to 12 mm in diameter: a tungsten carbide drill is the right tool for drilling all kinds of composite parts. On the market this drill is also called a "solid diamond drill". Drills with a sharp point angle (90 to 118°) or a brad point give better edge quality.
  • Holes larger than 12 mm: a diamond drill or diamond hole saw.
Drilling composites with a tungsten carbide drill and a diamond drill
Drilling composites: a tungsten carbide drill for diameters up to 12 mm and a diamond drill for larger ones; the hole surface after sanding and resin sealing.

Engineering tips for drilling composite parts

  • Wooden backing: placing a wooden backing under the composite part while drilling greatly improves the quality of the hole's exit edge and prevents fiber breakout and fraying.
  • Spindle speed: on hand drills and drill presses, a drill speed of about 300 to 1200 rpm is usually chosen; larger drills run slower. On CNC machines with carbide or PCD drills, higher speeds with a controlled feed can be used.
  • Feed force: high axial force as the drill breaks through is the main cause of delamination. Reduce the pressure near the end of the hole.
  • Heat: for deep holes, withdraw the drill several times to clear dust and cool it; dust building up in the drill flutes increases friction and heat.
  • Hole spacing: in bolted connections, the distance from the hole center to the edge of the part is usually at least about 2 to 3 times the hole diameter, and the spacing between holes about 4 times the diameter, to prevent edge tear-out.
  • Finishing and sealing: after drilling, smooth the hole wall with fine sandpaper and carefully coat it with resin using a small brush so the cut fibers are protected from moisture.

Guide to choosing the drill and speed for drilling composites

The table below is a practical guide to drilling composites with a drill press or hand drill. For larger diameters, a lower speed is chosen to control edge heat and keep the resin from burning:

Hole diameter (mm)Drilling toolApproximate speed (rpm)Recommendation
3 to 6Tungsten carbide drill900 to 1200Light, even feed
6 to 12Brad-point tungsten carbide drill600 to 900Wooden backing under the part
12 to 30Diamond drill or hole saw400 to 600Water cooling
Over 30Diamond hole saw300 to 400Drill from both sides of the part to prevent chipping

When drilling composites for bolted connections, the hole diameter is usually about 1 to 2 mm larger than the bolt diameter to absorb dimensional tolerance and thermal expansion. For high-volume drilling, a drill jig guarantees accurate hole positions and keeps the drill from wandering on the smooth surface of the profile.

Controlling dust when cutting and drilling

Dust from cutting and drilling composites consists of fine glass fiber and resin particles. It causes skin itching and irritation of the eyes and airways, and in large accumulations it is combustible. To control dust: connect power tools to an industrial vacuum with a HEPA filter, cut wet where possible, provide local or general ventilation, wear a filtering respirator (at least FFP2) and safety glasses, and never clean up dust with compressed air. After work, remaining dust on the bench is collected with a vacuum.

Milling and turning composite parts

Milling composite parts

Because fibers fray during milling, this type of machining is recommended for composite profiles only when necessary. If milling is needed, use carbide or diamond tools at high speed. "Compression" routers, which combine up-cut and down-cut flutes, push the fibers on the top and bottom surfaces inward and prevent fraying on both faces.

Milling speed for composite parts: vc ≈ 100 – 400 m/min

Turning composite parts

Turning composite parts such as polymer rods and fiberglass tubes is usually not recommended, because the longitudinal fibers are cut and the surface quality is poor. If necessary, turning with carbide tools is possible, and speeds and tool geometry are broadly similar to machining aluminum and brass:

Turning parameterRecommended value
Tool materialCarbide (preferably PCD for high volumes)
Turning speedAbout 400 m/min
Rake angle (cutting edge)10 to 15°
Depth of cutSmall; light passes to reduce fiber fraying
Engineering note: turning and milling cut the longitudinal surface fibers and remove the protective resin layer. In structural parts this reduces load capacity and creates a path for moisture ingress, so machined surfaces must always be coated with resin or paint.

Punching composite parts

Punching composite parts and the hole quality after punching
Punching composite parts — a fast way to make many holes in thin sheets and profiles.

Punching is a fast method for making many holes in thin sheets and profiles. Engineering tips for punching composite parts:

  • The maximum part thickness for punching is about 10 mm; in thicker parts the impact zone is crushed and radial cracks form.
  • A punch of hardened tool steel or carbide is recommended; a carbide punch lasts much longer against abrasive fibers.
  • Because of the material's elastic recovery, the hole produced is about 0.05 to 0.1 mm smaller than the punch diameter.
  • Small clearance between punch and die gives a cleaner edge.

Sanding composites

Sanding composites, before and after
Sanding composites: the surface before and after sanding with an orbital sander.
Grinding composite parts with an angle grinder is prohibited
Grinding the surface of composite parts with an angle grinder is prohibited; it burns the fibers and damages the part.
PurposeAbrasive type and grit
Shaping, removing chipping and preparing for bondingPaper sandpaper, grit 40 to 80
Preparing the surface for paintingSandpaper, grit 120 to 180
Smooth, polished surfaceWet-and-dry paper, grit 200 and up
Final glossPolisher and polishing compound; polish at low speed to avoid heating the surface
Warning: grinding with an angle grinder and grinding disc, because of the high heat and uncontrolled material removal, pulls out fibers, burns the resin and seriously damages parts. For sanding, use an orbital or random-orbit sander.

Can composite parts be welded?

Technically, thermoset composite parts (such as pultruded profiles with polyester and vinyl ester resin) cannot be welded, because after curing the polymer chains of these resins are linked into a three-dimensional network that does not melt with heat but decomposes. Composite parts are joined in two ways: mechanical joining with bolts and nuts, self-tapping screws and rivets, and chemical joining, i.e. bonding. Combining the two (a hybrid joint) gives the best performance. Only thermoplastic-matrix composites can be welded thermally, ultrasonically or by induction.

Joining composite parts with bolts, nuts and rivets

Joining composite parts with bolts and nuts, self-tapping screws and rivets
Types of mechanical joint for composite parts: bolts and nuts for load-bearing connections, self-tapping screws for low-stress connections, and rivets.
  • Bolts and nuts: for load-bearing connections, stainless or galvanized steel bolts and nuts, or composite bolts for corrosive and insulating environments, with wide washers to spread the pressure on the composite surface.
  • Self-tapping screws: for connections under low stress, such as covers and lids.
  • Rivets: steel and aluminum rivets for joining sheets and light parts.
Failure modes of bolted joints in composites: bolted joints in composite parts can fail in four modes: bearing of the hole wall, net-tension of the remaining section, shear-out between the hole and the edge, and cleavage. Sufficient edge distance, wide washers and controlled tightening torque (to avoid crushing the composite) prevent these modes. In bolted connections of hollow profiles, a sleeve or internal filler stops the wall of the composite box section from being crushed as the bolt is tightened.

When riveting composite parts or fitting pins, it is recommended to make the hole slightly larger than the rivet or pin and coat the joint with epoxy adhesive; this fills the gap and increases joint strength.

Bonding composite parts

Chemical joining with adhesive, alongside mechanical joining with bolts and nuts, gives composite joints ideal properties. Bonding spreads the load over a larger area, eliminates stress concentration around holes and seals the joint. Suitable adhesives for bonding composite parts are:

Adhesive typeFeatureApplication
Two-part epoxyHigh strength, low shrinkage, good chemical resistance, fairly brittle behaviorStructural and load-bearing connections
Two-part polyurethaneHigh flexibility and toughness, tolerates impact and vibrationConnections under vibration and differential thermal expansion
Methacrylate (MMA)Fast cure, less surface preparation neededFast assembly in production
Bonding composite parts with two-part epoxy and polyurethane adhesive
Bonding composite parts with two-part epoxy or polyurethane adhesive; applying the adhesive with a brush, spatula or mixing syringe.

Bonding steps

  1. Sanding: abrade the bonding area with coarse sandpaper (grit 40 to 80) to remove the glossy release layer
  2. Cleaning: clean the bonding area thoroughly of grease and dust with water, acetone and detergent
  3. Mixing: mix the two parts (adhesive and hardener) exactly in the specified ratio and in small amounts
  4. Applying: spread the adhesive on both surfaces with a brush, spatula or by hand (with gloves)
  5. Fixing: apply even pressure to both sides of the joint with clamps
  6. Curing: do not move the joint until it has reached sufficient strength

Common mistakes in bonding composite parts

  • Bonding to an unsanded surface: the release layer on the profile surface reduces adhesion several times over; the main cause of adhesive joint failure.
  • Wrong adhesive-to-hardener ratio: adding too much or too little hardener leaves the adhesive under-cured and the joint weak. The mix ratio must be measured with scales or a graduated syringe.
  • Bonding at low temperature or high humidity: below 10 °C, the adhesive cure stops or is incomplete.
  • Too thick an adhesive layer: adhesive thicker than about 2 mm has more voids and residual stress and lowers joint strength.
  • Moving too early: loading an adhesive joint before it has cured sufficiently breaks the fresh bond.

Technical tips for bonding with epoxy

  • Common epoxy adhesives gel in less than 50 minutes at ambient temperature (about 25 °C); after 24 hours they reach about 70 percent of their bond strength and maximum strength after about 7 days.
  • The temperature at the bonding site should be above 10 °C; the higher the temperature, the shorter the cure time.
  • The optimum adhesive layer thickness is usually about 0.2 to 0.5 mm, and the maximum should not exceed about 2 mm.
  • Estimate the amount of adhesive to mix according to the joint area; mixed adhesive has a limited working life.
  • For special parts that need very high joint strength, covering the joint with several layers of fiber and resin by hand lay-up is recommended. This turns the joint into a single integral part.
Designing an adhesive joint: adhesives are strong in shear and compression and weak in peel and through-thickness tension. So the joint should be designed so that the load is transferred mainly in shear — for example a lap joint, double-lap joint or scarf joint. Increasing the overlap length raises capacity up to a point. The shear strength of composite adhesive joints is usually evaluated by ASTM D5868.

Mechanical properties of a joint bonded with two-part epoxy

Joint propertyTypical value
Minimum tensile strength30 MPa
Minimum tensile modulus4500 MPa
ElongationLess than 1 percent
Joint service temperature−40 to +80 °C

Bonding versus mechanical joining

CriterionBondingBolts, nuts and rivets
Stress distributionEven over the whole bonded areaConcentrated around the hole
Need for drillingNoneYes; fibers are cut
Sealing the jointFullNeeds a sealant
Can be dismantledNoneYes
Sensitivity to surface preparationVery high; bond quality depends on sanding and cleaningLow
Quality controlHarder; bonding must be controlled to the procedureSimple (torque control)

For critical joints, combining bonding with bolts (a hybrid joint) is recommended: the bond provides stiffness and sealing, and the bolts provide a second load path if the adhesive is damaged. Before bonding, surfaces must be free of dust; even a thin layer of sanding dust greatly reduces joint strength. After final polishing, any remaining polishing compound is also wiped off with acetone before painting or bonding.

Painting composite surfaces

Polyester and vinyl ester resins are inherently vulnerable to ultraviolet radiation. Outdoors, after a while the surface of composite parts becomes dull and chalky, changes color and the surface fibers show through (fiber blooming). So for composite parts installed outdoors, painting with a UV-resistant coating is recommended. The steps for painting composite parts are:

  1. Cleaning: clean the part surface thoroughly with detergent and acetone
  2. Abrading: roughen the surface with sandpaper (grit 120 to 180) to improve paint adhesion
  3. Primer (optional): for ideal quality, spray an epoxy primer onto the surface
  4. Drying: let the primer set and dry according to the instructions
  5. Topcoat: spray a polymer paint made for composites at the correct mix ratio
  6. Finishing: check the appearance and paint adhesion
Painting composite surfaces with polyurethane and epoxy paint
Painting composite surfaces with polyurethane and epoxy paints for UV protection.
Yellow, white and grey colored composite fiberglass sheet
Colored composite sheets — color can be added to the resin during production or applied by painting after installation.
Paint typeFeatureUse in painting composites
Aliphatic polyurethaneExcellent UV resistance, retains color and glossOutdoor topcoat
EpoxyExcellent adhesion and chemical resistance, poor UV resistancePrimer and coating for indoor chemical environments
Polyester (gelcoat)Fully compatible with a polyester substrateRepair and surface coating

For parts that are both bonded and painted, bond first and paint after the adhesive has fully cured, because adhesive does not stick well to a painted surface. Each coat of paint is usually 40 to 60 microns thick, and 1 to 2 coats are applied depending on the quality required. Paint adhesion can be checked with the cross-cut test to ISO 2409.

Important: pultruded profiles contain internal mold release, which leaves a slippery layer on the surface. Without sanding and cleaning with acetone, no paint or adhesive will stick properly. Never skip this step.

Summary table of machining parameters for composite parts

OperationRecommended toolSpeed or key parameterMain point
Cutting compositesDiamond or carbide blade (200 to 500 mm diameter)1800 to 3600 m/minSlow feed, part free of vibration, coolant
Drilling compositesTungsten carbide drill up to 12 mm; diamond drill for largerAbout 300 to 1200 rpm (by hand)Wooden backing, less pressure at breakthrough
MillingCarbide or diamond cutter, compression router100 to 400 m/minOnly when necessary
TurningCarbide tool, rake angle 10 to 15°About 400 m/minPoor surface quality; recoat the surface
PunchingHardened steel or carbide punchMaximum thickness about 10 mmHole 0.05 to 0.1 mm smaller than the punch
SandingGrit 40 to 80 for shaping, 200 and up for finishingOrbital or random-orbit sanderNo grinding with an angle grinder
BondingTwo-part epoxy, polyurethane or methacrylateAdhesive thickness up to about 2 mmSanding and cleaning with acetone
PaintingEpoxy primer and polyurethane topcoat40 to 60 microns per coatAbrade the surface before painting

Cutting and preparing products at Nabak Composite

At Nabak Composite, profiles are cut to standard or custom lengths with diamond saws after leaving the pultrusion line. To learn about the production process, read the pultrusion process, and for the dimensional accuracy of cut length and angle, read dimensional tolerances of pultruded products. Our team can also advise on choosing the right adhesive and paint for bonding and painting composite parts.

The Nabak Composite production team on the pultrusion line
The Nabak Composite production team adjusting reinforcing mat on the pultrusion line.
Nabak Composite pultrusion line and surface veil feed
Surface veil on the Nabak production line; after cutting, this protective layer is cut through at the edges, which is why edge sealing matters.

The tips in this article on cutting, drilling and bonding apply to all Nabak composite products — from composite box sections, fiberglass angles, composite channels and composite beams to composite flat bars, polymer rods, composite wire, composite grating and cable trays:

Composite box sectionsCut with a diamond blade; internal sleeve in bolted joints.
Fiberglass anglesDrill with a carbide drill and respect edge distances.
Composite channelsBolted joints combined with bonding.
Composite beamsDrilling the web and flange for structural connections.
Fiberglass tubeSquare cut with a V clamp.
Composite flat barsFast punching and drilling.
Polymer rods and composite wireCut with a hacksaw or diamond disc.
Composite grating and fiberglass sheetCut with a diamond saw and seal the edges.
Cable trays and laddersJoined with stainless steel bolts and nuts.

Frequently asked questions about cutting and machining composites

What is the best blade for cutting composites?

For cutting composites, a diamond blade or a carbide-tipped blade is the best choice; the blade diameter is 200 to 500 mm depending on part thickness, and the peripheral speed about 1800 to 3600 m/min.

What drill should I use to drill composites?

For holes up to 12 mm, a tungsten carbide drill (sold as a "solid diamond drill") is recommended, and for larger diameters a diamond drill or diamond hole saw. A wooden backing under the part prevents fiber fraying at the hole exit.

Can composite parts be welded?

No; thermoset composite parts do not melt and cannot be welded. They are joined mechanically, with bolts, nuts and rivets, or chemically, by bonding.

What is the best adhesive for bonding composite parts?

Two-part epoxy, polyurethane and methacrylate adhesives are suitable for bonding composite parts. At 25 °C, epoxy adhesive reaches about 70 percent of its strength after 24 hours and full strength after about 7 days.

Why are outdoor composite parts painted?

Polyester and vinyl ester resins are vulnerable to ultraviolet radiation and over time change color and expose their surface fibers; painting with a UV-resistant polyurethane coating protects the surface.

Summary

Cutting and other machining operations on composite parts are easy to do to a high standard with the right tools and a few simple principles. Tungsten carbide and diamond tools, a slow and even feed, holding the part without vibration, support at the exit of cuts and holes, and sealing edges with resin are the keys to quality cutting and drilling. Milling and turning should be done only when necessary, grinding with an angle grinder is prohibited, and thermoset parts cannot be welded; they are joined with bolts, nuts, rivets and epoxy or polyurethane bonding. Finally, painting with a polyurethane coating ensures the durability of composite parts outdoors. For advice on choosing the right tools, adhesive and paint, contact the Nabak Composite team.

Nabak Composite

This article was prepared by the technical team of Nabak Composite, a manufacturer of pultruded composite profiles and products.