Manufacturing processes technical articles | Nabak Composite

What Is Hand Lay-Up? An Engineering Guide to Making Fiberglass Parts by Manual Lamination

Hand lay-up is the simplest and yet the most widely used method of making composite parts, but the quality of the final part depends on dozens of technical details. In this guide we review the whole hand lay-up chain, from making the pattern and mold to gel coat, laying up fiber, de-airing, curing, finishing and producing fiberglass sheet, together with calculations of thickness and resin-to-fiber ratio.

Publisher: Nabak Composite Topic: Composite manufacturing processes Reading time: about 15 minutes

What is the hand lay-up method?

Hand lay-up, also known as manual lamination, wet lay-up and hand laminating, is an open molding method. In this method, reinforcing fibers are laid layer by layer on the mold surface, wetted with resin, and consolidated and de-aired with a roller. After the resin cures at ambient temperature, the composite part is released from the mold.

Hand lay-up is the best solution for making large or complex fiberglass and composite parts in low to medium volumes — from boat hulls, tanks and ducts to vehicle parts, kiosks and fiberglass sheet. Its initial investment is very low and there is no limit on part size. However, despite its simple appearance, hand lay-up involves many technical points which, if ignored, severely reduce the quality and durability of the final part.

Hand lay-up raw materials: reinforcing glass fiber, resin matrix and additives
The three main groups of materials in hand lay-up: reinforcing fibers, resin (matrix) and additives.

Main materials in hand lay-up

Material groupCommon examplesRole in the part
Reinforcing fibersChopped strand mat (CSM), woven roving (WR), woven fabric, tissueCarrying load and determining strength and stiffness
Resin (matrix)Polyester, vinyl ester, epoxyBinding fibers, transferring load, chemical resistance
AdditivesCatalyst (MEKP), cobalt accelerator, color paste, filler, UV and fire-retardant additivesControlling cure, color, resistance and special properties
Surface materialsGel coat, top coatAppearance and surface protection
Auxiliary materialsRelease wax, PVA film, silicone sprayEasy release of the part from the mold

The three main stages of hand lay-up production

To make a composite product by hand lay-up, a mold of the part must be prepared, and making the mold requires a physical model (pattern) of the part. The only exception is a metal mold, which is CNC-machined directly without a pattern. So the production chain has three stages:

1 Making the pattern (model) A one-to-one replica of the part CNC, 3D printing, sculpting 2 Making the mold Taking a mold from the pattern Composite, silicone, foam, plaster 3 Making the part Hand lay-up Gel coat, fiber, resin, de-airing
The three main stages of hand lay-up: making the pattern, making the mold and making the part by hand lay-up.

Stage one: making the pattern (model)

The pattern, or model, is a real 3D replica of the final product made at one-to-one scale. Every surface defect in the pattern is carried exactly into the mold and then into every part, so the pattern's surface quality sets the ceiling for the quality of the composite parts. In other words, an accurate pattern and mold are prerequisites for producing quality composite parts, and every hour spent finishing the pattern pays off in all subsequent parts. With advances in technology, achieving an accurate pattern is easier than before. Pattern-making methods fall into two broad groups:

CriterionIndustrial (mechanized) methodsArtistic (manual and improvised) methods
TechnologiesCNC machining, 3D printing, 3D optical scanning and reverse engineeringSculpting, template making, turning and hand forming
Dimensional accuracyVery high and repeatableDepends on the maker's skill
SpeedHighLow to medium
CostHigherLower
LimitationLimited by machine size and materialLimited accuracy on complex geometry

In industrial pattern-making, the 3D model is first designed in software (or an existing part is captured with a 3D scanner) and then built by 3D printing or CNC machining from a foam or wood block. In artistic methods such as sculpting and template making, the maker's experience and taste make it possible to create varied and organic patterns.

Pattern materials: paper and cardboard, various foams including urethane foam (rigid urethane modeling foams) and polyurethane foam, polystyrene foam (EPS), clay (modeling clay), plaster and wood. Clay suits organic forms and sculptural patterns, but its surface must be fully sealed before molding. The surfaces of porous patterns such as foam, plaster and wood must be filled with putty and primer, then sanded and polished before molding.

Engineering points in pattern-making:
  • Draft angle: vertical walls should have at least 1 to 3 degrees of draft so the part releases from the mold without sticking.
  • Corner radii: sharp corners (radius less than about 3 mm) cause fibers to bridge away from the surface and bubbles to form in the corner.
  • Readiness for mold-making: before making the mold, the pattern must be completely dry, polished and waxed.
  • Shrinkage: polyester resin shrinkage is significant at large sizes and must be compensated for in precise patterns.
  • Surface sealing: the styrene in resin dissolves polystyrene foam (EPS); before molding, the surface of this foam must be isolated with a resistant coating.

Stage two: molding and mold-making

Mold-making is the most expensive and time-consuming part of production preparation. Taking a mold from the pattern is the second stage of making a part by hand lay-up. The mold material and quality are chosen according to production volume, part size, required surface quality and budget. Before molding, the pattern surface is coated with release agent using silicone spray or special waxes so that the mold separates easily from the pattern. Mold types in hand lay-up are:

Plaster mold (single-use)The plaster mold is broken to remove the part; suitable when only one part is needed.
Foam moldMade mainly from polyurethane foam formed from two components, isocyanate and polyol (follow the isocyanate-to-polyol mix ratio in the manufacturer's datasheet), and needs repair after every few uses.
Silicone moldFlexible and suitable for small parts with fine details and undercuts; its life depends on part size, resin type and silicone quality.
Metal moldMade directly by CNC machining without a pattern; because of its high cost, it is less common in hand lay-up.
Composite moldThe most common mold in hand lay-up and the most common molding method; made from the pattern using the same technique of laying up fiber and tooling gel coat.
Mold typePattern needed to make the moldApproximate production volumeCost to makePart surface quality
Plaster moldYes1 partVery lowModerate
Polyurethane foam moldYesA few to a few dozen parts (with repair)LowModerate
Silicone moldYesDozens of parts (small parts)ModerateGood, with fine detail
Composite moldYesHundreds of parts (with proper maintenance)ModerateExcellent (glossy)
Metal moldNone (CNC)Thousands of partsVery highExcellent

Making a composite mold: this molding method is the most widely used. On the waxed pattern, a layer of tooling gel coat, which is harder and more resistant than ordinary gel coat, is applied first. Then layers of fiber and low-shrink resin are laid up to a thickness usually two to three times that of the part. For large molds, a reinforcing frame of steel profile or composite profile is attached to the back of the mold so it does not warp over its life. Before the first production run, the mold surface is waxed and polished several times. The quality of mold-making is reproduced directly in the appearance and dimensional accuracy of every part, so mold-making is no place to economize.

Stage three: the hand lay-up steps

Once the mold is ready, the part is made by hand lay-up in the following steps. The order of these steps is the same as the order of layers in the part's cross-section:

  1. Wax: waxing the mold surface with release wax
  2. Release agent: applying PVA film or silicone spray
  3. Gel coat: applying a layer about half a millimeter thick
  4. Tissue: a layer of tissue to reinforce the gel coat
  5. Lay-up: resin and fiber to the required thickness
  6. De-airing: consolidating the layers with a suitable roller
  7. Final layer: finer fiber for an even back surface
  8. Top coat: if required
Mold surface (composite, metal or silicone) Release wax + PVA film Gel coat — wet thickness about 0.5 mm Surface tissue to reinforce the gel coat First layer of chopped strand mat (CSM) — corrosion barrier Intermediate layers: chopped strand mat and woven roving (WR) Final layer of finer fiber for an even surface Top coat (optional) Order of application from the bottom (mold surface) up
Schematic cross-section of a composite part made by hand lay-up; layers in order of application from the mold surface up.

1 and 2. Preparing the mold: wax and release film

The clean, dry mold surface is waxed with several coats of release wax (usually carnauba-based), polishing after each coat. Then, for extra assurance, PVA (polyvinyl alcohol) release film is applied by spray or sponge as a thin, even layer; for simpler parts silicone spray can be used. New or repaired molds need more coats of wax.

3. Applying gel coat

Gel coat is a layer of thickened, pigmented resin that forms the outer surface of the part. Its main components are base resin, fumed silica (Aerosil) for thixotropy and to prevent sagging on vertical walls, talc powder as filler, and color paste. The amounts of Aerosil and talc must be balanced; too much filler reduces the gel coat's resistance to water and weathering. Gel coat is applied to the mold by brush or spray gun to a wet thickness of about 0.4 to 0.5 mm.

When to start lay-up: after applying the gel coat, wait until it has gelled but not fully hardened. A simple workshop test: if you touch the gel coat surface with a gloved hand and it does not stick (but is still slightly soft), it is the right time to start lay-up. Starting earlier causes the gel coat to wrinkle from the styrene in the next layer's resin (alligatoring), and starting later causes poor adhesion and delamination.

4. Tissue layer

A layer of surface tissue (veil) with plenty of resin is placed behind the gel coat. This thin layer reinforces the gel coat, prevents the texture of coarse fibers showing on the surface (print-through) and creates a resin-rich layer for chemical resistance.

Surface tissue to reinforce gel coat in hand lay-up
Surface tissue (veil): reinforces the gel coat and prevents fiber print-through.

5. Laying up fiber and resin

Before starting, the fiber is cut to suitable sizes and the resin is prepared by adding catalyst (usually MEKP at 1 to 2 percent of resin weight). First a coat of resin is applied to the surface, then the fiber is laid and the resin is worked into it with a brush or roller. The number of layers is set by the required thickness. The edges of each layer should overlap the adjacent layer by about 25 to 50 mm, and joints should be staggered in successive layers.

Chopped strand mat (CSM) for hand lay-up
Chopped strand mat (CSM): the most used reinforcement for fiberglass parts in hand lay-up.
Fiberglass woven roving
Woven roving: to increase strength in the intermediate layers.

6. De-airing with a roller

De-airing is the most important quality step in hand lay-up. Grooved metal rollers or nap rollers consolidate the fiber and resin layers to expel trapped air bubbles and fully wet the fibers. Every remaining bubble is a point of stress concentration and a site where cracks and delamination start; each percent of porosity reduces interlaminar shear strength by about 5 to 10 percent.

Composite microstructure of glass fiber, resin matrix and an air void from incomplete de-airing
Laminate microstructure: glass fibers, resin matrix and a void (bubble); de-airing with a roller is essential to remove voids.

7 and 8. Final layer and top coat

In the last layer, finer fiber (such as light mat or tissue) is used so the back of the part is neat and even and no sharp fibers stick out. If needed, a top coat is applied to the back surface. Top coat contains paraffin wax, which isolates the surface from air and allows full, tack-free surface cure.

Important points in hand lay-up production

The importance of gel coat for part durability

The life, durability and appearance of most composite parts depend on their surface layer, the gel coat. To achieve properties such as resistance to ultraviolet light, scratch and abrasion resistance, and chemical resistance, the gel coat formulation and additives are decisive. The main ingredient of gel coat is resin, chosen according to the required chemical or physical properties from polyester (isophthalic or isophthalic/NPG), vinyl ester or epoxy, and it can contain anti-abrasion and anti-UV additives. In outdoor parts, UV absorbers in the gel coat prevent yellowing and chalking of the surface.

Gel coat parameterRecommended valueConsequence if out of range
Wet thickness0.4 to 0.5 mmToo thin: incomplete cure and fiber show-through; too thick: star cracks
Consumption400 to 600 g/m²—
MEKP catalyst1.5 to 2.5 percentToo little: incomplete cure; too much: brittleness and discoloration
Workshop temperature18 to 30 °CCold: slow cure; hot: rapid gelling and a wavy surface

Controlling cure reaction heat

Polyester resin cure is an exothermic reaction, and the thicker the wet laminate, the more heat is trapped in its core. In hand lay-up with chopped strand mat, if there are more than four or five layers, the resin should be allowed to gel or partly harden before applying further layers, to avoid the ill effects of excessive heat (warping, cracking, scorching and discoloration of the resin, and fiber print-through on the gel coat). In thick parts, low-exotherm resins and less catalyst are used.

Releasing the part from the mold

Once the required weight or thickness is reached and the resin has cured sufficiently, the part is released from the mold. For fiberglass parts with complex shapes, compressed air or high-pressure water blown through valves built into the mold or from the edges can release the part without damage. Using a metal lever scratches the mold surface and is not allowed; plastic wedges together with compressed air are the safe release method.

Finishing and trimming

The final step is finishing and trimming excess resin and fiber from around the part. This is best done with a knife before the part fully hardens, when the resin has gelled but not yet reached final hardness (green trim); after hardening, trimming is done with a diamond disc or grinder. When using a grinder, dust extraction and a respirator are essential. Cut edges should be sealed with resin so moisture does not penetrate the fibers. Read about tools and methods in the article cutting composites.

Cutting a fiberglass composite part with a diamond disc
Trimming excess with a diamond disc.
Finishing and sanding the surface of a composite part
Finishing and sanding the surface of a composite part.

Engineering calculations: resin-to-fiber ratio and layer thickness

In hand lay-up with chopped strand mat, the resin-to-fiber weight ratio (R) is usually 2 to 2.5. With this ratio, fiber weight fraction and thickness per layer are calculated as follows:

Wf = 1 / (1 + R)   |   t (mm) = mf × (1/ρf + R/ρm) / 1000

where Wf is the fiber weight fraction, mf the fiber weight per unit area (g/m²), ρf the density of glass fiber (2.55 g/cm³) and ρm the density of cured resin (about 1.2 g/cm³). For R between 2 and 2.5, the fiber weight fraction is about 29 to 33 percent. The table below is calculated for common reinforcements:

Fiber typeFiber weight (g/m²)Resin-to-fiber ratioResin used (g/m²)Thickness per layer (mm)
Chopped strand mat CSM 3003002.3~700~0.70
Chopped strand mat CSM 4504502.3~1050~1.05
Chopped strand mat CSM 6006002.3~1400~1.40
Woven roving WR 6006001.0~600~0.74
Woven roving WR 8008001.0~800~0.98
Worked example:To make a panel with a laminate thickness of 4 mm using CSM 450:
  • Number of layers: 4 ÷ 1.05 ≈ 3.8 → 4 layers of CSM 450 (thickness ≈ 4.2 mm)
  • Fiber used: 4 × 450 = 1800 g/m²; laminate resin: 1800 × 2.3 ≈ 4140 g/m²
  • Gel coat: about 500 g/m²; total part weight ≈ 6.4 kg/m²
  • Four layers can be applied wet-on-wet; greater thicknesses need staged application after gelling.

Reducing the resin-to-fiber ratio (i.e. increasing fiber content) through better de-airing and the use of woven roving increases strength and stiffness, but dry spots must be carefully controlled. To predict mechanical properties from fiber content, see the article predicting the properties of polymer composites.

Types of glass fiber for hand lay-up: chopped strand mat and woven fabric
Chopped strand mat and woven fabric; the fiber type determines the resin ratio and thickness of each layer.

Common defects in hand lay-up production and how to prevent them

Most defects in composite parts made by hand lay-up originate in one of the process steps and can be prevented by process control. The table below summarizes the most common defects of this method:

DefectMain causePrevention
Bubbles and porosityIncomplete de-airing with the rollerThorough rolling of each layer, resin of suitable viscosity
Dry spotsInsufficient resin or premature gellingControlling gel time and resin per layer
Gel coat wrinkling (alligatoring)Starting lay-up before the gel coat has gelled, or gel coat too thinTouch test and 0.4 to 0.5 mm thickness
Pre-release from the moldToo much wax, excessive heat or shrinkageControlling heat and the number of wet-on-wet layers
Fiber print-throughNo tissue layer, fast cureUsing a tissue layer and low-shrink resin
DelaminationLong delay between layers, surface contaminationSanding the hardened layer surface before continuing
Gel coat star cracksThick gel coat or impactControlling gel coat thickness
BlisteringOsmotic water penetration through unsuitable gel coatIsophthalic/NPG or vinyl ester gel coat in wet environments

Producing fiberglass sheet by hand lay-up

The steps for making fiberglass sheet by hand lay-up in various thicknesses and colors are similar to the part production process, except that instead of a mold, a flat surface such as glass or Melinex (polyester) film is used. Once the resin has dried, the Melinex film is peeled from the top surface of the fiberglass sheet (the film leaves the sheet surface smooth and glossy), and excess fiber and resin is trimmed with a suitable cutting tool such as a grinding disc.

In fiberglass roofing sheets, as thickness and number of layers increase, the heat generated during resin cure also increases; this heat causes uneven shrinkage, and tension must be applied to the film to prevent creasing and wrinkling of the sheet surface. Besides looking poor, creases are sites of stress concentration and water penetration. Fiberglass composite sheets, also known as fiberglass roofing sheet, can be produced in rolls or sheets 1 to 3 m wide; rolls suit long coverings and sheets suit standard sizes. The weight of fiberglass roofing sheet is determined by the number of layers and the fiber weight.

Sinusoidal (corrugated) and trapezoidal fiberglass sheet are produced like flat sheet, except that a galvanized sheet with a sinusoidal or trapezoidal profile of the required pitch and height is used as the mold for forming. The choice of pitch and profile height determines the sheet's bending stiffness and the allowable spacing of supports (purlins).

Flat, corrugated sinusoidal and trapezoidal fiberglass sheet made by hand lay-up
Flat, sinusoidal (corrugated) and trapezoidal fiberglass sheet.
Corrugated sinusoidal fiberglass sheet
Sinusoidal fiberglass sheet: formed on a corrugated galvanized mold.
Trapezoidal fiberglass sheet for roofing
Trapezoidal fiberglass sheet for roof and wall cladding.

For technical specifications, thicknesses and properties of fiberglass sheet types, read the article technical specifications of fiberglass and plastic roofing sheet.

Comparing hand lay-up with other composite production methods

The choice of production method depends on volume, size, surface quality and the required mechanical properties. The table below shows where hand lay-up stands alongside other methods:

Manufacturing methodFiber weight fractionMold costSuitable volumeSmooth surface
Hand lay-up30 to 45%LowLow to mediumOne side
Spray-up25 to 35%LowModerateOne side
Vacuum infusion55 to 70%Low to mediumLow to mediumOne side
RTM45 to 60%HighMedium to highBoth sides
Pultrusion60 to 80%HighContinuous mass productionAll surfaces

Advantages of hand lay-up: very low investment and mold cost, no size limit, ability to make complex parts, local reinforcement with extra layers, and a variety of colors and gel coats. Limitations: quality depends on operator skill, lower fiber content, one smooth surface, slower for mass production, and styrene vapor emissions in the workplace.

Safety in the hand lay-up workshop

In the manual method, the operator is in direct contact with resin, catalyst and fiber. Styrene vapor, skin contact with peroxide catalyst and fiber dust during cutting are the main hazards. Local ventilation, a respirator with organic vapor filters, nitrile gloves, safety goggles and suitable workwear are mandatory, and catalyst must never be mixed directly with cobalt accelerator. See more details in the article safety in composite products.

Personal protective equipment in hand lay-up: respirator, goggles, gloves and workwear
Personal protective equipment in a hand lamination workshop.

Nabak Composite and fiberglass products

Drawing on technical know-how in pultrusion and lay-up processes, Nabak Composite produces and supplies composite parts, composite products and fiberglass sheet. Sinusoidal, trapezoidal and flat fiberglass sheet in various thicknesses and numbers of layers is available in the required lengths and widths, in rolls or sheets.

Flat fiberglass sheetColored, clear and gel-coated.
Sinusoidal fiberglass sheetCorrugated sheet for roofs and walls.
Trapezoidal fiberglass sheetFor sheds and canopies.
FRP profiles and gratingPultruded and molded.
Nabak Composite red and black colored fiberglass sheet
Nabak Composite colored fiberglass sheets, available in rolls or sheets.

Frequently asked questions about hand lay-up

What is the hand lay-up method?

Hand lay-up is an open molding method in which reinforcing fibers are laid layer by layer on a mold, wetted with resin and de-aired with a roller, and after cure the composite part is released from the mold. It is the best option for large, complex parts in low to medium volumes.

How thick is the gel coat in hand lay-up?

The wet thickness of gel coat is usually about 0.4 to 0.5 mm, with consumption of about 400 to 600 g/m². Thinner gel coat does not protect the surface against UV and abrasion, and thicker gel coat is prone to cracking.

What is the resin-to-fiber ratio in hand lay-up?

For chopped strand mat (CSM), the resin-to-fiber weight ratio is usually 2 to 2.5, i.e. a fiber weight fraction of about 29 to 33 percent. For woven roving, the ratio falls to about 1 to 1.2.

How many layers can be applied in succession by hand?

Usually no more than four or five layers of chopped strand mat should be applied wet-on-wet, because the heat of the resin cure reaction rises and causes warping, cracking and scorching. After that number, the resin should be allowed to gel before further layers are applied.

What is the most common mold in hand lay-up?

The composite (fiberglass) mold is the most common mold in hand lay-up, and is itself made from the pattern by the same lay-up technique. Silicone, polyurethane foam, plaster and metal molds are also used depending on volume and part size.

Summary

Hand lay-up, with its three stages of pattern-making, mold-making and manual lamination, is the most flexible and lowest-cost method of making composite and fiberglass parts. The final quality of the part depends on the details reviewed in this guide: accuracy and surface quality of the pattern, choosing a mold suited to the volume, preparing the mold with wax and PVA, gel coat of the right thickness and correct timing, a tissue layer, a resin-to-fiber ratio of 2 to 2.5 for chopped strand mat, thorough de-airing with a roller, controlling cure heat in multiple layers, and timely trimming and finishing. Following these principles gives a durable, attractive part with reliable mechanical properties. For advice on fiberglass products, contact the Nabak Composite team.

Nabak Composite

This article was prepared by the technical team of Nabak Composite, a manufacturer of composite products and fiberglass sheet.