Predicting the Properties of Polymer Composites: From Fiber Volume Fraction to the Rule of Mixtures — An Engineering Calculation Guide with Worked Examples

In this article we learn how to predict composite properties without making and testing the final part, using only the properties of the fibers and resin and their proportions: calculating density, converting weight fraction to volume fraction, estimating void volume fraction, and longitudinal and transverse modulus and strength with the rule of mixtures and the Halpin-Tsai equations, with a complete worked example for a pultruded profile.

Publisher: Nabak Composite Topic: Composite micromechanics Reading time: about 25 minutes

Why does predicting composite properties matter?

When designing any product from polymer composites, the engineer must know before making the mold and setting up the production line what stiffness, strength, weight and thermal behavior the final part will have. Making specimens and testing every possible combination of fiber and resin is both costly and time-consuming. Fortunately, a branch of materials mechanics called micromechanics makes it possible to predict the properties of a composite with acceptable engineering accuracy from the technical data of its constituents — the properties of the fibers, the properties of the resin and their proportions.

These calculations play a key role at three stages: in preliminary design, to choose the type of fiber, type of resin and their proportions; in quality control, to compare test results with the theoretical value and detect defects such as voids or fiber shortage; and in cost optimization, to find the minimum amount of fiber that meets the technical requirements. Below we go through these formulas step by step with a worked example for a composite profile made of glass fiber and polyester resin.

Constituents of polymer composites: glass fiber, glass mat and fabric, and polyester resin as matrix
The constituents of a polymer composite: glass fiber as roving, mat and fabric as reinforcement, and polyester resin as matrix. The properties of the final composite are predicted from the combined properties of these constituents.

Input data needed to predict composite properties

In composite materials theory, polymer composites are treated as a set of separate constituents whose mechanical properties are each known. So to calculate the properties of composite materials using micromechanics formulas, we need three kinds of information:

  • Fiber properties: density, tensile modulus, tensile strength, elongation at break, Poisson's ratio and coefficient of thermal expansion. These data are given in the fiber manufacturer's datasheet.
  • Cured resin properties: density, tensile and flexural modulus, tensile and flexural strength, elongation and coefficient of thermal expansion. These values are usually obtained from tests on cast specimens of neat resin (cast resin).
  • Amount and arrangement of constituents: weight or volume fraction of fiber and resin, fiber orientation (unidirectional, bidirectional or random) and void content.

Weight fraction and volume fraction: the two bases of composite calculations

The most important factor in determining a composite's properties is the type and amount of its constituents. The amount of each constituent can be expressed on two bases:

Weight fraction: the ratio of the weight of each constituent to the total weight of the composite:

wf = Wf / Wc   ,   wm = Wm / Wc   ,   wf + wm = 1

Volume fraction: the ratio of the volume of each constituent to the total volume of the composite:

Vf = vf / vc   ,   Vm = vm / vc   ,   Vf + Vm + Vv = 1

Weight fraction is easily measured experimentally. The most common method is the resin burn-off test according to ASTM D2584 or ISO 1172: a specimen of the composite part is weighed and placed in a furnace at about 560 to 600 °C until the resin matrix burns away completely, and the remaining fiber is then weighed. The ratio of fiber weight to the specimen's initial weight gives the fiber weight fraction. Note that mineral fillers such as calcium carbonate also remain after burning and must be accounted for separately.

By contrast, volume fraction is the parameter used in micromechanics theory and formulas, because mechanical behavior depends on the cross-section occupied by each constituent, not on its weight. Converting weight fraction to volume fraction is therefore the first step in any composite property prediction:

Vf = (wf / ρf) / [ (wf / ρf) + (wm / ρm) ]   |   wf = Vf·ρf / ρc
Important note: because the density of glass fiber (about 2.55) is roughly twice that of resin (about 1.2), the fiber volume fraction is always noticeably lower than its weight fraction. For example, 60 percent glass fiber by weight occupies only about 42 percent of the composite volume. Confusing the two is one of the most common errors in composite calculations.

Calculating the density of composites

The theoretical density of a composite can be calculated from the volume or weight fractions of its constituents:

From volume fraction:

ρc = Vf·ρf + Vm·ρm

From weight fraction:

ρc = 1 / [ (wf / ρf) + (wm / ρm) ]

So to calculate composite density, all we need are the densities of the fiber and resin and their proportions. The first relation is a simple rule of mixtures, and the second comes from summing the partial volumes. Both give the same result for a void-free composite. For composites containing filler, the filler term (wp/ρp) is also added to the denominator.

Measuring composite density by immersion

The actual density of a part is measured by immersion, or Archimedes' principle, according to ASTM D792. The specimen is weighed once in air and once immersed in distilled water, and density is calculated from:

ρexp = [ Wair / (Wair − Wwater) ] × ρwater
Measuring composite density by immersion according to ASTM D792
Immersion test to measure the actual density of a composite specimen; the specimen is weighed suspended in water, and the difference between its weight in air and in water gives its volume and therefore its density.

Void volume fraction: an indicator of composite production quality

In practice, the measured density of a composite part is always slightly lower than the theoretical density. The difference is due to voids in the part, caused by air trapped between fibers, incomplete wet-out, resin volatiles or shrinkage. The lower the void volume fraction, the more complete the fiber wet-out and the higher the product quality. According to ASTM D2734, void volume fraction is calculated from:

Vv = 1 − ( ρexp / ρth ) = ( ρth − ρexp ) / ρth

In high-quality composites (such as autoclave-cured aerospace parts) void volume fraction is below 1 percent, and in industrial pultruded products it is usually about 1 to 3 percent. Each percent of voids can reduce interlaminar shear strength and flexural strength by several percent.

Microstructure of a polymer composite with glass fibers, resin matrix and a void
Micrograph of a composite cross-section: glass fibers (light circles), resin matrix and a void. Analyzing these images, or micro-tomography, is the direct method of determining void volume fraction.

A second, more accurate method for determining void volume fraction is micro computed tomography (micro-CT). In this non-destructive method, hundreds of X-ray images are taken from different angles and a 3D model of the internal structure is built, also showing the distribution, size and shape of the voids. A third method is image analysis of polished sections under an optical or electron microscope.

The rule of mixtures: the basis for predicting composite mechanical properties

In composite materials theory, the simplest and most widely used theory for predicting the properties of polymer composites is the rule of mixtures. It rests on several basic assumptions:

  • The fibers are long, continuous, parallel and uniform (same diameter and properties);
  • The fibers are evenly distributed in the matrix;
  • There is a perfect bond without slip between fiber and resin;
  • The composite has no voids;
  • Under longitudinal load, fiber and matrix have equal strain (the iso-strain or Voigt model).

Longitudinal tensile modulus (along the fibers)

Assuming equal strain, the total stress equals the volume-fraction-weighted average of the stresses, and the longitudinal modulus is given by:

E11 = Vf·Ef + Vm·Em

This relation is very accurate for longitudinal modulus (usually less than 5 percent error), because along the fibers the iso-strain assumption holds almost exactly.

Transverse tensile modulus (perpendicular to the fibers)

Perpendicular to the fibers, the constituents carry load "in series", and the equal stress assumption (Reuss model) leads to the inverse rule of mixtures:

1 / E22 = Vf / Ef + Vm / Em

This relation underestimates the transverse modulus. For a more accurate prediction, the semi-empirical Halpin-Tsai equations are used:

E22 = Em · (1 + ξ·η·Vf) / (1 − η·Vf)   ,   η = (Ef/Em − 1) / (Ef/Em + ξ)

The shape factor ξ for circular fibers is usually taken as 2 when calculating transverse modulus.

Poisson's ratio, shear modulus and coefficient of thermal expansion

Major Poisson's ratio:

ν12 = Vf·νf + Vm·νm

In-plane shear modulus (lower estimate):

1 / G12 = Vf / Gf + Vm / Gm   ,   G = E / [2(1+ν)]

Longitudinal coefficient of thermal expansion (Schapery equation):

α11 = (Ef·αf·Vf + Em·αm·Vm) / (Ef·Vf + Em·Vm)

Longitudinal tensile strength

Predicting strength is more complex than predicting modulus, because it depends on the order in which the constituents fail. When the failure strain of the resin is greater than or close to that of the fiber (as with glass fiber and a tough polyester resin), longitudinal strength is estimated from:

σc ≈ Vf·σf + Vm·σ'm

where σ'm is the stress in the matrix at the moment of fiber failure (at most equal to the resin strength). At typical volume fractions the fibers contribute more than 90 percent of the strength, and the simpler estimate σc ≈ Vf·σf can also be used.

Effect of fiber volume fraction on composite elastic modulus (E-glass fiber and polyester resin)

Longitudinal modulus E₁₁ — rule of mixtures Transverse modulus E₂₂ — Halpin-Tsai Transverse modulus E₂₂ — inverse rule of mixtures
0 10 20 30 40 50 60 0% 20% 40% 60% 80% Fiber volume fraction (Vf) Elastic modulus (GPa) Vf = 0.42 Longitudinal (rule of mixtures) — Vf=0% : 3.8 GPa Longitudinal (rule of mixtures) — Vf=10% : 10.7 GPa Longitudinal (rule of mixtures) — Vf=20% : 17.6 GPa Longitudinal (rule of mixtures) — Vf=30% : 24.6 GPa Longitudinal (rule of mixtures) — Vf=40% : 31.5 GPa Longitudinal (rule of mixtures) — Vf=50% : 38.4 GPa Longitudinal (rule of mixtures) — Vf=60% : 45.3 GPa Longitudinal (rule of mixtures) — Vf=70% : 52.2 GPa Longitudinal (rule of mixtures) — Vf=80% : 59.2 GPa Longitudinal (rule of mixtures) in the worked example: 32.7 GPa Transverse (Halpin-Tsai) — Vf=0% : 3.8 GPa Transverse (Halpin-Tsai) — Vf=10% : 4.9 GPa Transverse (Halpin-Tsai) — Vf=20% : 6.2 GPa Transverse (Halpin-Tsai) — Vf=30% : 7.8 GPa Transverse (Halpin-Tsai) — Vf=40% : 9.8 GPa Transverse (Halpin-Tsai) — Vf=50% : 12.4 GPa Transverse (Halpin-Tsai) — Vf=60% : 15.9 GPa Transverse (Halpin-Tsai) — Vf=70% : 21.0 GPa Transverse (Halpin-Tsai) — Vf=80% : 28.8 GPa Transverse (Halpin-Tsai) in the worked example: 10.2 GPa Transverse (inverse mixture) — Vf=0% : 3.8 GPa Transverse (inverse mixture) — Vf=10% : 4.2 GPa Transverse (inverse mixture) — Vf=20% : 4.7 GPa Transverse (inverse mixture) — Vf=30% : 5.3 GPa Transverse (inverse mixture) — Vf=40% : 6.1 GPa Transverse (inverse mixture) — Vf=50% : 7.2 GPa Transverse (inverse mixture) — Vf=60% : 8.8 GPa Transverse (inverse mixture) — Vf=70% : 11.3 GPa Transverse (inverse mixture) — Vf=80% : 15.7 GPa Transverse (inverse mixture) in the worked example: 6.3 GPa Longitudinal E₁₁ Transverse E₂₂ (Halpin-Tsai) Transverse E₂₂ (inverse mixture)

The chart above shows a key fact: increasing the fiber volume fraction raises the longitudinal modulus linearly and steeply, but the transverse modulus stays close to that of the resin until high volume fractions. That is why unidirectional composites are strongly anisotropic, and in products such as pultruded profiles, layers of mat and fabric are used to provide transverse properties.

Complete worked example: predicting the properties of a composite profile

To see the formulas in practice, we predict the properties of a composite profile made by pultrusion from E-glass fiber and unsaturated polyester resin. To simplify the calculations, we assume the part consists only of fiber and resin, and that the weight of additives such as catalyst and filler is included in the resin weight.

Step 1: input data

In this worked example we apply all the formulas introduced, in order, to a real composite profile. The mechanical properties of the constituents are as follows:

PropertyUnsaturated polyester resin (cured)E-glass fiber
Density ρ1.22 g/cm³2.55 g/cm³
Tensile modulus E3800 MPa73000 MPa
Flexural modulusapprox. 3650 MPa—
Tensile strength σ80 MPa2400 MPa (effective roving value)
Flexural strengthapprox. 130 MPa—
Elongation at breakapprox. 3%approx. 4.8%
Poisson's ratio ν0.350.22
Coefficient of thermal expansion αapprox. 70 × 10⁻⁶ /°Capprox. 5 × 10⁻⁶ /°C

Part composition: one profile length with a final weight of 1000 g, comprising 600 g of glass fiber and 400 g of resin with additives. These figures vary for each composite product depending on cross-section shape and production method.

Step 2: fiber and resin weight fractions

wf = 600 / 1000 = 0.60   ,   wm = 400 / 1000 = 0.40

Step 3: converting to volume fraction

Fiber volume = 600 ÷ 2.55 = 235.3 cm³ and resin volume = 400 ÷ 1.22 = 327.9 cm³; total volume = 563.2 cm³.

Vf = 235.3 / 563.2 = 0.418   ,   Vm = 0.582

That is, 60 percent fiber by weight makes up only about 42 percent by volume of the part.

Step 4: calculating composite density

ρc = 1 / (0.60/2.55 + 0.40/1.22) = 1 / 0.5632 = 1.776 g/cm³

Check with the volume fraction relation: 0.418 × 2.55 + 0.582 × 1.22 = 1.066 + 0.710 = 1.776 ✓

Step 5: estimating void volume fraction

Suppose the specimen's density measured by immersion is 1.73 g/cm³:

Vv = 1 − 1.73 / 1.776 = 0.026 → 2.6%

This value is within the acceptable range for industrial pultruded profiles. If the void volume fraction exceeds about 3 to 4 percent, line speed, resin viscosity and fiber wet-out quality should be reviewed.

Step 6: longitudinal and transverse tensile modulus

E11 = 0.418 × 73000 + 0.582 × 3800 = 30514 + 2212 ≈ 32.7 GPa
E22 (Reuss) = 1 / (0.418/73000 + 0.582/3800) ≈ 6.3 GPa
E22 (Halpin-Tsai, ξ=2) ≈ 10.2 GPa

Step 7: Poisson's ratio, shear modulus and thermal expansion

ν12 = 0.418 × 0.22 + 0.582 × 0.35 ≈ 0.30
Gf ≈ 29.9 GPa , Gm ≈ 1.41 GPa → G12 ≈ 2.3 GPa
α11 ≈ 9.4 × 10⁻⁶ /°C

Interestingly, the predicted longitudinal coefficient of thermal expansion (about 9 µm/m/°C) is close to that of steel (about 12) and concrete — one reason composite profiles create little thermal stress alongside concrete and metal structures.

Step 8: longitudinal tensile strength

σc ≈ 0.418 × 2400 + 0.582 × 80 ≈ 1003 + 47 ≈ 1050 MPa (theoretical upper bound)

This is the theoretical upper bound for a perfectly unidirectional, flawless composite. In the next section we will see why the actual value is lower and why calculating real mechanical properties requires correction factors.

Summary of predicted composite properties

Predicted propertySymbolValueCalculation method
Fiber volume fractionVf41.8%Conversion from weight fraction
Theoretical composite densityρc1.78 g/cm³Volume rule of mixtures
Void volume fraction (with ρexp=1.73)Vv2.6%ASTM D2734
Longitudinal tensile modulusE1132.7 GPaRule of mixtures
Transverse tensile modulusE226.3 to 10.2 GPaReuss / Halpin-Tsai
Shear modulusG122.3 GPaInverse rule of mixtures
Poisson's ratioν120.30Rule of mixtures
Longitudinal coefficient of thermal expansionα119.4 × 10⁻⁶ /°CSchapery equation
Longitudinal tensile strength (upper bound)σcapprox. 1050 MPaRule of mixtures

From a single ply to a real profile: the effect of mat and fiber orientation

Real pultruded profiles are not made of unidirectional fibers alone; they combine layers of roving (unidirectional) with continuous filament mat or fabric (for transverse properties). Two tools are used to predict the properties of such a section:

1. Krenchel orientation efficiency factor: the effect of fiber orientation is introduced into the rule of mixtures with a factor η0:

Ec = η0·Vf·Ef + Vm·Em
Fiber arrangementEfficiency factor η0 (in the principal direction)Example form
Unidirectional (roving)1Pultruded rebar and flat bar
Balanced bidirectional 0/90°0.5Woven fabric
Random in-plane0.375Chopped strand mat and continuous filament mat
Random 3D0.2Chopped fibers in injection-molded parts

2. Through-thickness averaging of layers (classical lamination theory approximation for symmetric in-plane loading):

Ex ≈ Σ ( tk · Ex,k ) / t

Example: if 75 percent of the thickness of a composite box section is a roving layer with a longitudinal modulus of 32.7 GPa and 25 percent is a mat layer with a modulus of about 9 GPa, the longitudinal modulus of the whole profile is predicted as about 0.75 × 32.7 + 0.25 × 9 ≈ 26.8 GPa. This is above the 23 GPa minimum required for grade E23 in EN 13706, so the designer can be reasonably confident, before the die is made, that the product will comply with the standard. For a more complete analysis, especially under bending and for unsymmetric laminates, the ABD matrices of classical lamination theory (CLT) are used.

Nabak Composite pultruded fiberglass tube with roving and mat layers
Section of Nabak composite tubes: the longitudinal fiber (roving) and mat layers are visible in the wall; the longitudinal and transverse properties of these tubes are predicted by combining the rule of mixtures with through-thickness averaging of layers.

Why do actual composite properties differ from theoretical predictions?

The rule of mixtures and micromechanical relations give an idealized picture of the material. In practice, measured mechanical properties always lie between the predicted longitudinal and transverse values and are usually below the theoretical upper bound. The main causes of this difference are:

FactorEffect on propertiesProduction remedy
VoidsReduced shear and flexural strength and fatigue resistanceControl of resin viscosity, line speed and wet-out
Fiber misalignment and wavinessSevere reduction in modulus and longitudinal compressive strengthUniform roving tension and precise preforming
Fiber damage during processingReduced effective fiber strengthCeramic guides and an abrasion-free fiber path
Incomplete fiber–resin adhesionReduced load transfer and transverse strengthSizing compatible with the resin
Uneven fiber distributionStress concentration and local property variationDesigning the fiber layout across the section
Thermal residual stress and incomplete cureMicrocracking and reduced long-term propertiesControl of the die temperature profile
Ambient temperature and humidityReduced matrix-dominated propertiesChoosing a suitable resin and design reduction factors

For this reason, engineers use overall efficiency factors for strength (usually 0.5 to 0.8 for industrial profiles) and characteristic values from tests for structural design. For example, with an orientation factor of about 0.8 for a section with roving and mat, and a factor of about 0.8 for fiber misalignment and damage, a realistic longitudinal tensile strength of about 0.64 × 1000 ≈ 650 MPa is estimated for a roving-rich section; in profiles with a larger share of mat, this figure is lower.

Golden engineering rule: no formula or theory on its own replaces testing. Predicting composite properties is for "design and selection" and experimental testing is for "verification". The best approach combines the two: first the optimum composition is chosen by calculation; then, with a limited number of tensile, flexural and density tests, the model is calibrated and used with greater confidence for subsequent designs.

Tests to verify composite properties

To validate the results of the formulas and calibrate the model, the mechanical and physical properties of composite materials are measured with the following standard tests:

PropertyTest standardUse in validating the prediction
Fiber weight fractionASTM D2584 / ISO 1172Main input to the calculations
DensityASTM D792Comparison with theoretical density
Void volume fractionASTM D2734 / Micro-CTIndicator of wet-out quality
Tensile strength and modulusASTM D638 / ISO 527-4Verification of E11 and σc
Flexural strength and modulusASTM D790 / ISO 14125Flexural behavior of the profile
Interlaminar shear strengthASTM D2344Quality of fiber–resin adhesion

Predicting composite properties at Nabak Composite

At Nabak Composite, the design of every new product starts with composite calculations: roving type and tex, the number and type of mat layers, fiber content and resin type are chosen so that the predicted properties match the project requirements and reference standards. The results are then validated by density, burn-off and mechanical tests on production specimens. To learn about fiber types and their properties, read the article types of fiber in composites.

Green fiberglass composite grating with predicted mechanical properties
Composite grating: its load capacity is calculated from the predicted properties of fiber and resin and the grid geometry.
Nabak gray fiberglass composite grating
Gray composite grating: fiber volume fraction and wet-out quality determine its stiffness and durability.
Polymer composite products including profiles, box sections, tubes and composite grating
The range of pultruded composite products, from unidirectional rebar and flat bar to box sections and grating with combined fiber layouts.

Frequently asked questions about predicting composite properties

What is the rule of mixtures in composites?

The rule of mixtures is a relation that predicts composite properties as the volume-fraction-weighted average of the properties of the fibers and resin; for example, longitudinal modulus equals Vf·Ef + Vm·Em.

What is the difference between fiber weight fraction and volume fraction?

Weight fraction is the ratio of fiber weight to the total weight of the part and is easily measured by a burn-off test; volume fraction is the ratio of fiber volume to total volume and is used in composite property prediction formulas. The two are converted using the densities of the fiber and resin.

How is composite density calculated?

The theoretical density of a composite equals one divided by the sum of each constituent's weight fraction divided by its density: ρc = 1 / (wf/ρf + wm/ρm). Actual density is measured by immersion according to ASTM D792.

How is void volume fraction determined?

Void volume fraction is obtained from the difference between theoretical and measured density: Vv = 1 − ρexp/ρth, according to ASTM D2734. Micro computed tomography is a more accurate, non-destructive method for this.

Why are actual composite properties lower than theoretical predictions?

Because of voids, fiber misalignment, fiber damage in production, incomplete fiber–resin adhesion, uneven fiber distribution and mat layers with random fibers; that is why efficiency factors and experimental tests are used.

Summary

Predicting the properties of polymer composites, and composite materials in general, is a powerful tool for designing composite products quickly and economically. From the properties of the fiber and resin and their weight fractions, one can calculate the fiber volume fraction, composite density, void volume fraction, longitudinal and transverse tensile modulus, shear modulus, Poisson's ratio, coefficient of thermal expansion and the upper bound of tensile strength. The rule of mixtures is very accurate for longitudinal properties, while the Halpin-Tsai equations should be used for transverse properties. Finally, the effects of fiber orientation, mat layers, voids and production defects must be accounted for with efficiency factors and experimental tests. For advice on designing and selecting the right composite product, contact the technical team at Nabak Composite.

Nabak Composite

This article was prepared by the technical team of Nabak Composite, a manufacturer of pultruded composite profiles and products.