Advanced Mechanics of Composite Materials and Structures
Advanced Mechanics of Composite Materials and Structures

Advanced Mechanics of Composite Materials and Structures

Advanced Mechanics of Composite Materials and Structures: A Comprehensive Book Summary

An advanced guide to FRP composite mechanics: unidirectional plies, angle-ply, fabric, lattice and 3D plies, laminates and failure criteria, environmental effects, creep, fatigue and impact, effects of the manufacturing process, and optimal structural design from filament-wound pressure vessels to anisogrid lattice structures

Authors of the original book: Valery V. Vasiliev, Evgeny V. Morozov
Publisher: Elsevier — field: mechanics and design of composite structures
Prepared for: NABAK Composite

What sets this book apart

This book is the product of decades of experience designing composite space and aircraft structures (especially filament-wound structures). What distinguishes it from common textbooks is its reliance on "applied mechanics for real design": extensive experimental data, frank discussion of the limitations of models, the nonlinear behavior of angle-ply layers, fabric and lattice layers, the effect of the manufacturing process (winding tension, residual stress, fiber waviness) and a unique section on optimal composite structures: uniform-strength laminates, isotensoid pressure vessels and anisogrid lattice structures.

How to use this summary

  • Orange "Key point" boxes give the most important engineering conclusion of each chapter.
  • Gold "Note" boxes show how the material applies to FRP products such as profiles, pipes, tanks and panels.
  • Notation: direction 1 is along the fibers, 2 perpendicular to the fibers; σ̄ is strength; φ is the fiber angle relative to the x axis.
  • Sample figures are given to convey scale and are no substitute for design and test data.
NABAK CompositePage 1 of 19
Advanced Mechanics of Composite Materials and Structures
Advanced Mechanics of Composite Materials and Structures

Table of Contents

  1. 1Introduction: structural materials and the place of composites
  2. 2Fundamentals of solid mechanics
  3. 3The unidirectional ply: stiffness and micromechanics
  4. 4The unidirectional ply: strength and failure modes
  5. 5Orthotropic and angle-ply layers
  6. 6Fabric, lattice and 3D layers
  7. 7Laminate stiffness
  8. 8Stress analysis, thermal effects and nonlinear laminate behavior
  9. 9Ply failure criteria
  10. 10Laminate strength and allowable stresses
  11. 11Effects of temperature and moisture
  12. 12Time-dependent behavior: creep, fatigue and impact
  13. 13Effects of the manufacturing process
  14. 14Optimal structures and pressure vessels
  15. 15Anisogrid lattice structures
  16. 16Conclusions and frequently asked questions
  17. 17Glossary
The book's main message in one sentenceThe best composite structure places the fibers exactly along the load path and relieves the matrix of load-bearing as far as possible; composite mechanics is a tool for achieving this "optimal fibrous structure".
NABAK CompositePage 2 of 19
Advanced Mechanics of Composite Materials and Structures
Advanced Mechanics of Composite Materials and Structures

1Introduction: structural materials and the place of composites

The book opens by comparing structural materials by specific strength (σ̄/ρ) and specific stiffness (E/ρ). Structural metals have almost the same specific modulus (about 25 Mm), whereas fibrous composites can offer several times that along the fibers.

MaterialDensity (g/cm³)Tensile strength (MPa)Modulus (GPa)
High-strength steel7.8~1500–2000210
Aluminum2.7~400–60072
Titanium4.5~1000110
Unidirectional glass/epoxy~2.1~1800~60
Unidirectional carbon/epoxy~1.55~2000–2500~140–180
Unidirectional aramid/epoxy~1.35~2000~90

Typical values in the fibre direction for high-quality unidirectional composites.

Why fibers?

The theoretical strength of materials is far higher than their actual strength, because defects and cracks create stress concentrations. Thin fibers, being small in volume, have fewer defects and a strength close to the theoretical value. To use this strength, the fibers are placed in a matrix that holds them together, transfers load, and brings broken fibers back into service.

The book's approach

  • From material to structure: unidirectional ply → angle-ply and fabric layers → laminate → optimal structure.
  • Grounded in experiment: every model is evaluated against real experimental data and its limits of validity are stated.
  • Attention to manufacturing: composite properties are formed in the structure itself and depend on the manufacturing method.
  • Optimal design: the ultimate aim is a structure in which all the fibers reach their strength limit simultaneously and uniformly.
Key pointThe real advantage of composites lies along the fibers; if a structure is designed so that the matrix carries a large part of the load, the composite will be no better than metal. The art of design is aligning the fibers with the load path.
NABAK CompositePage 3 of 19
Advanced Mechanics of Composite Materials and Structures
Advanced Mechanics of Composite Materials and Structures

2Fundamentals of solid mechanics

Before turning to composites, the book briefly reviews the fundamentals of continuum mechanics, focusing on what composite analysis needs.

Stress, equilibrium and strain

∂σx/∂x + ∂τxy/∂y + ∂τxz/∂z + qx = 0    (and cyclic)    εx = ∂u/∂x, γxy = ∂u/∂y + ∂v/∂x

Stress and strain transformation under axis rotation, principal stresses and compatibility equations are reviewed. These transformations underpin the analysis of off-axis plies.

Constitutive equations

  • Anisotropic linear elasticity: generalized Hooke's law with up to 21 constants; symmetry of the compliance matrix (νᵢⱼ/Eᵢ = νⱼᵢ/Eⱼ).
  • Nonlinear elasticity and elastoplasticity: for matrices and plies under shear; deformation theory and flow theory of plasticity.
  • Viscoelasticity: the Boltzmann–Volterra hereditary theory with creep and relaxation kernels.
  • Thermal: free thermal strains and the heat conduction equation.

Variational principles

Π = U − W → min    (minimum total potential energy)     Castigliano / minimum complementary energy

The principles of minimum potential energy and complementary energy give upper and lower bounds on the effective stiffness of heterogeneous materials and underpin the Ritz and finite element approximate methods. The book uses these principles in micromechanics and structural analysis.

Why does this chapter matter for composites?

  • Composites behave differently in different directions (elastic, nonlinear, viscoelastic); the appropriate constitutive model must be chosen for each direction.
  • Interlaminar and through-thickness stresses, neglected in plate theories, are recovered from the 3D equilibrium equations.
  • Most numerical solutions for composite structures are built on variational principles.
Key pointIn composites, the "linear elastic" assumption always holds only along the fibers; for shear and transverse matrix loading, nonlinear and time effects can matter at working stress levels.
NABAK CompositePage 4 of 19
Advanced Mechanics of Composite Materials and Structures
Advanced Mechanics of Composite Materials and Structures

3The unidirectional ply: stiffness and micromechanics

Fibers and matrix

The book compares glass, carbon, aramid, boron and high-molecular-weight polyethylene fibers, and polymer (thermoset and thermoplastic), metal, ceramic and carbon matrices, in terms of mechanical properties and stress-strain behavior. An important point: the failure strains of the fiber (about 0.5 to 3 percent) and matrix must be compatible, so the matrix does not crack before the fibers.

Ply structure and volume fraction

Fiber arrangement in a real ply is random and is approximated by square or hexagonal models. The maximum theoretical volume fraction for circular fibers is about 0.785 (square) and 0.907 (hexagonal); in practice about 0.5 to 0.7.

Micromechanics of stiffness

E₁ = E_f·V_f + E_m·V_m    ν₂₁ = ν_f·V_f + ν_m·V_m
1/E₂ = V_f/E_f + V_m/E_m    1/G₁₂ = V_f/G_f + V_m/G_m    (lower estimates)

The book stresses that micromechanical models, especially for E₂ and G₁₂, are highly sensitive to geometric and interface assumptions and are suitable only for understanding trends. Carbon and aramid fibers are also anisotropic, with a transverse modulus far lower than their longitudinal modulus; using the fiber's longitudinal modulus in the E₂ formula causes a large error.

The phenomenological approach

Rather than relying fully on micromechanics, the book recommends determining ply properties by direct testing of unidirectional plies or filament-wound tubes and using them as a homogeneous orthotropic material. Micromechanics is used to analyze the effect of changing V_f and to select materials.

Ply (V_f ≈ 0.6)E₁ (GPa)E₂ (GPa)G₁₂ (GPa)ν₂₁
Glass/epoxy~60~13~3.4~0.3
Carbon/epoxy~140~11~5.5~0.27
Aramid/epoxy~95~5~2~0.34
Key pointFor design, take ply properties from direct testing, not micromechanics; micromechanics is a tool for understanding and improving materials, not a substitute for test data.
NABAK CompositePage 5 of 19
Advanced Mechanics of Composite Materials and Structures
Advanced Mechanics of Composite Materials and Structures

4The unidirectional ply: strength and failure modes

Longitudinal tension

Tensile failure of a unidirectional ply is a statistical process: weaker fibers break first, the matrix transfers load back into them over an ineffective length, and final failure occurs through accumulation and clustering of breaks. Fiber strength decreases with length (Weibull distribution), so fiber strength in a composite is higher than in a dry bundle. The book shows that fiber–matrix bond quality and uniform fiber tension during manufacture strongly affect tensile strength.

Longitudinal compression

Failure modes: fiber microbuckling in the matrix, shear failure and longitudinal splitting. Compressive strength depends on matrix shear modulus, initial fiber misalignment and bonding:

σ̄₁⁻ ≈ G_m / (1 − V_f)    (shear microbuckling, ideal), reduced strongly by fibre waviness

Experimental data are much lower than this prediction and sensitive to the test method. Aramid fibers have low compressive strength because of their fibrillar structure.

Transverse tension and compression and in-plane shear

  • Transverse tension: stress concentration in the matrix between fibers; cracks parallel to the fibers; low strength (tens of MPa).
  • Transverse compression: shear failure on an inclined plane; strength several times the transverse tensile strength.
  • In-plane shear: strongly nonlinear matrix behavior; strength depends on how it is defined (strain limit).

Hybrid composites

Combining fibers with different failure strains (for example carbon and glass) in one ply or laminate: the lower-strain fibers break first; if their fraction is small, the other fibers carry the load and failure becomes more gradual (the hybrid effect).

Strength (MPa) – approximateGlass/epoxyCarbon/epoxy
σ̄₁⁺ longitudinal tension~1300–1800~1500–2300
σ̄₁⁻ longitudinal compression~600–900~900–1200
σ̄₂⁺ transverse tension~30–40~40–60
σ̄₂⁻ transverse compression~130–150~150–250
τ̄₁₂ shear~50–70~60–90
Key pointThe unidirectional ply is "single-purpose": very strong along the fibers and weak in other directions. Transverse and shear strengths are tens of times lower than longitudinal strength, and design should not rely on them for significant load.
NABAK CompositePage 6 of 19
Advanced Mechanics of Composite Materials and Structures
Advanced Mechanics of Composite Materials and Structures

5Orthotropic and angle-ply layers

The orthotropic ply in rotated axes

A unidirectional ply at angle φ to the x axis behaves anisotropically in the x-y system, with tension-shear coupling. The modulus in the x direction:

1/E_x = cos⁴φ/E₁ + (1/G₁₂ − 2ν₂₁/E₁)·sin²φ·cos²φ + sin⁴φ/E₂

The angle-ply layer (±φ)

A symmetric layer made of equal numbers of +φ and −φ plies (such as filament-wound layers) is orthotropic in its plane; the shear coupling of each sub-ply is cancelled by the opposite sub-ply. Stiffnesses:

A₁₁ = Ē₁cos⁴φ + Ē₂sin⁴φ + 2Ē₁₂sin²φcos²φ    A₄₄ = (Ē₁ + Ē₂ − 2Ē₁ν₁₂)sin²φcos²φ + G₁₂cos²2φ

(Ēᵢ = Eᵢ/(1−ν₁₂ν₂₁), Ē₁₂ = Ē₁ν₁₂ + 2G₁₂). The Poisson's ratio of a ±φ layer can be very large (over 1), even though the Poisson's ratio of each individual sub-ply is small.

Nonlinear behavior of angle-ply layers

One of the book's signature topics: in a ±45 layer under tension, load is carried mainly by in-plane shear in the matrix and the stress-strain curve is strongly nonlinear. At large strains the fibers rotate toward the load direction (the angle decreases) and stiffness rises again. The book presents models based on nonlinear shear behavior and geometric change, and shows that a linear model badly underestimates strain in these layers.

Edge effects and interlaminar stresses in angle-ply layers

In flat ±φ specimens, interlaminar shear stresses arise near the edges, so tests on flat specimens show lower strength than filament-wound tubes (which have no free edges). That is why the book recommends tubular specimens for characterizing ±φ layers.

Angle φDominant behavior
0° to about 15°Fiber-controlled; almost linear
About 30° to 60°Matrix shear dominates; nonlinear; large Poisson's ratio
About 75° to 90°Controlled by matrix transverse tension; brittle
Key point±φ layers at intermediate angles are excellent for shear and torsional stiffness but behave nonlinearly and matrix-dependently in tension; do not design them to carry the main tensile load.
NABAK CompositePage 7 of 19
Advanced Mechanics of Composite Materials and Structures
Advanced Mechanics of Composite Materials and Structures

6Fabric, lattice and 3D layers

Fabric layers

In woven fabrics (plain, satin, twill), warp and weft fibers cross over each other, creating fiber curvature (crimp). Consequences:

  • Lower in-plane stiffness and strength than an equivalent cross-ply laminate with straight fibers (especially in compression).
  • Better resistance to delamination and impact damage, and better drapeability on curved molds.
  • In tension, straightening of the wavy fibers causes nonlinear behavior at the start of loading.

The book presents models based on fiber wave geometry for calculating fabric stiffness, and also covers triaxial and stitched fabrics.

Lattice layers

A layer of spaced unidirectional ribs, with no skin or a thin skin. Each rib carries load only along its own axis (monotropic model). The equivalent layer stiffness is found by averaging the ribs' contributions. This concept underpins anisogrid lattice structures (chapter 15).

Spatially reinforced (3D) composites

Fibers in three (or more) directions by 3D weaving, stitching or inserted rods. Advantages: high delamination resistance, damage tolerance and through-thickness load capacity. Drawbacks: lower in-plane fiber volume fraction, fiber curvature and high cost. Typical uses: carbon-carbon composites and thick structures.

Isotropic and short-fiber layers

Layers with short fibers or random mat are almost isotropic in-plane; their stiffness is estimated by averaging unidirectional ply properties over all angles (about one third of the unidirectional ply's longitudinal stiffness).

Note for FRP productsPultruded profiles combine unidirectional layers (roving) with random or fabric layers (mat and stitched fabric); with the models in this chapter, the stiffness of each wall can be calculated from the contributions of these layers.
Key pointThe straighter and more aligned the fibers, the higher the in-plane stiffness and strength; the more interlaced they are (fabrics, 3D), the greater the resistance to damage and delamination. Choosing the layer type is a trade-off between the two.
NABAK CompositePage 8 of 19
Advanced Mechanics of Composite Materials and Structures
Advanced Mechanics of Composite Materials and Structures

7Laminate stiffness

The general anisotropic laminate

Assuming Kirchhoff kinematics and perfect bonding between plies, force and moment resultants are related to the strains and curvatures of a reference surface:

{N; M} = [[B, C], [C, D]]·{ε; κ}    B_mn = Σ A_mn⁽ⁱ⁾(tᵢ − tᵢ₋₁), C_mn = ½Σ A_mn⁽ⁱ⁾(tᵢ² − tᵢ₋₁²), D_mn = ⅓Σ A_mn⁽ⁱ⁾(tᵢ³ − tᵢ₋₁³)

(Vasiliev–Morozov notation: B membrane, C coupling, D bending; equivalent to A, B, D elsewhere.)

The book shows that by choosing the reference surface appropriately (for example one that makes C₁₁ zero), some couplings can be eliminated; but in general not all couplings can be eliminated at once. The real magnitude of coupling is measured by the "reduced bending stiffness" D − C²/B.

Special laminates

TypeFeature
SymmetricC = 0 about the mid-plane; no in-plane–bending coupling
OrthotropicMade of 0 and 90 plies and balanced ±φ pairs; no shear coupling
Quasi-homogeneousMany thin repeated plies: C ≈ 0 and D ≈ B·h²/12; behaves like a homogeneous plate
Quasi-isotropice.g. repeated [0/±60] or [0/±45/90]; in-plane stiffness independent of direction
SandwichStiff faces and a light core; bending stiffness from face separation and shear from the core

The quasi-homogeneous laminate

The book considers this concept important: when different plies are alternated and repeated many times, the laminate can be treated as a homogeneous anisotropic material with bending stiffness proportional to its in-plane stiffness. Many filament-wound and pultruded structures are close to this case, which simplifies their analysis.

The quasi-isotropic laminate

Its in-plane modulus is roughly one third to two fifths of the unidirectional ply's longitudinal modulus; that is why the book stresses that using quasi-isotropic laminates as a "black metal" throws away much of the advantage of composites.

Key pointA quasi-homogeneous laminate with thin repeated plies practically eliminates couplings and simplifies analysis; in layup design, repeating and dispersing plies is better than stacking plies of the same orientation together.
NABAK CompositePage 9 of 19
Advanced Mechanics of Composite Materials and Structures
Advanced Mechanics of Composite Materials and Structures

8Stress analysis, thermal effects and nonlinear laminate behavior

Stress analysis

By solving the constitutive equations for known loads, the reference surface strains and curvatures, the strain in each ply and then the stress in material axes are calculated. For quasi-homogeneous filament-wound and pultruded laminates, ply stresses come directly from the in-plane strains.

Thermal stresses

σ₁⁽ⁱ⁾ = Ē₁(ε₁ + ν₁₂ε₂) − Ē₁(α₁ + ν₁₂α₂)ΔT, …    N^T = Σ ∫ (thermal terms) dz

The book gives numerical examples of residual thermal stresses after cure: in cross-ply and angle-ply laminates, the transverse tensile stress from cooling can on its own use up a large part of the transverse strength and cause matrix cracks even without load. The thermal expansion of carbon ±φ laminates can be negative; this property is used to design dimensionally stable structures (antennas and space mirrors).

Nonlinear behavior of laminates

  • Material nonlinearity: nonlinear shear behavior of plies in laminates with ±φ plies; analyzed by iterative methods (secant or tangent stiffness).
  • Matrix cracking before failure: as transverse plies crack, their transverse and shear stiffness drop but the fibers still carry longitudinal load; the laminate behaves piecewise linearly.
  • Geometric nonlinearity: fiber rotation at large strains in angle-ply layers.

The monotropic (netting) model

At high strains where the matrix has cracked, it can be assumed that only the fibers carry load along their own direction (E₂ = G₁₂ = 0). This simple model, which the book evaluates against experimental data from filament-wound structures, is very accurate for predicting ultimate strength and for preliminary design of optimal fibrous structures.

N_x = h·σ̄₁·Σ ψᵢ cos²φᵢ    N_y = h·σ̄₁·Σ ψᵢ sin²φᵢ    N_xy = h·σ̄₁·Σ ψᵢ sinφᵢcosφᵢ

ψᵢ is the thickness fraction of plies at angle φᵢ.

Key pointThe two models are complementary: the full elastic model (with matrix) for stiffness and damage onset, and the monotropic model (fibers only) for the ultimate strength of fibrous structures with a suitable layup.
NABAK CompositePage 10 of 19
Advanced Mechanics of Composite Materials and Structures
Advanced Mechanics of Composite Materials and Structures

9Ply failure criteria

The book reviews failure criteria critically and empirically, distinguishing two groups: "polynomial" criteria that approximate the failure surface with a smooth function, and "structural" criteria that assess fiber and matrix failure modes separately.

Main criteria

CriterionFeature
Maximum stress / maximum strainSimple; identifies the failure mode; no interaction
Quadratic (Tsai-Hill, Hoffman, Tsai-Wu)A smooth surface; stress interaction; interaction coefficients need biaxial tests
Hashin, Puck and mechanism-based criteriaSeparating fiber and matrix failure; matrix failure on an inclined plane

The book's practical recommendation

For the unidirectional ply, experimental data show that the interaction of longitudinal stress σ₁ with σ₂ and τ₁₂ is weak. The following combination is therefore recommended:

fibre failure: σ₁ = σ̄₁⁺ (tension) or |σ₁| = σ̄₁⁻ (compression)
matrix failure: (σ₂/σ̄₂)² + (τ₁₂/τ̄₁₂)² = 1    (σ̄₂ = σ̄₂⁺ or σ̄₂⁻ by sign; refined forms for compression)

In transverse compression, compressive stress increases the apparent shear strength, and more refined criteria (such as fracture-plane-based criteria) account for this effect.

The book's critical points

  • No single criterion covers all the data; the World-Wide Failure Exercise showed this.
  • Polynomial criteria may predict unrealistic strength for some load cases.
  • Shear and transverse strength data are sensitive to the test method (flat or tubular specimen).
  • For fabric layers, criteria must be calibrated with data for that particular fabric.
Key pointChoose a simple, mechanism-based failure criterion: maximum stress for the fibers and a quadratic criterion for the matrix. Making the criterion more complex without valid biaxial data does not improve accuracy.
NABAK CompositePage 11 of 19
Advanced Mechanics of Composite Materials and Structures
Advanced Mechanics of Composite Materials and Structures

10Laminate strength and allowable stresses

Progressive laminate failure

  1. Linear laminate analysis and applying the failure criterion to each ply.
  2. Determining first-ply failure load; usually matrix cracking in transverse or angle plies.
  3. Degrading the damaged ply's properties: for matrix cracking, E₂ and G₁₂ are reduced (or zeroed); the fibers still carry load.
  4. Re-analysis until fiber failure in the main plies (ultimate failure).

Through experimental comparison, the book shows that for laminates with fibers along the load path, ultimate strength is well predicted by the monotropic model and first-ply failure load by the elastic model.

Allowable stresses and strains

The book discusses setting allowable stress frankly:

  • Safety factors: larger than for metals, because of greater data scatter, brittle behavior and sensitivity to damage and environment.
  • Matrix failure limit: in structures where leakage or environmental ingress matters (tanks, pipes), matrix cracking is itself treated as failure, and working stress must stay below first-ply failure load.
  • Strain-based design: limiting the working strain of the fibers (for example to below about 0.3 to 0.5 percent in aircraft applications) to cover damage, environment and fatigue.
  • Statistical values: design strength with a specified survival probability from the statistical distribution of the data.

The probabilistic approach

Composite strength has significant scatter. The book introduces a method of determining structural reliability from statistical distributions of strength and load: in large structures with a large volume of material, the probability of a defect is higher and effective strength lower (the size effect).

Interlaminar stresses

At free edges, holes, ply drops and joints, interlaminar stresses and delamination are an independent failure criterion not captured by laminate theory; 3D analysis or fracture mechanics criteria are needed.

Key pointFirst decide what "failure" means for the structure: for tanks and pipes, matrix cracking and leakage; for a dry load-bearing structure, fiber failure. This choice changes the allowable stress several-fold.
NABAK CompositePage 12 of 19
Advanced Mechanics of Composite Materials and Structures
Advanced Mechanics of Composite Materials and Structures

11Effects of temperature and moisture

Temperature

  • High temperature: as the matrix glass transition temperature is approached, transverse and shear moduli and matrix-controlled strengths fall sharply; longitudinal properties are more stable.
  • Low and cryogenic temperatures: the matrix becomes stiffer and more brittle; residual thermal stresses increase with further cooling and cause matrix microcracks. For cryogenic fuel tanks, matrix cracking and leakage are the main issue.
  • Thermal cycling: accumulation of microcracks due to the difference in α between fiber and matrix.

Thermal properties

α₁ ≈ (E_f·α_f·V_f + E_m·α_m·V_m)/E₁    λ₁ = λ_f·V_f + λ_m·V_m    (conductivity along fibres)

The longitudinal expansion coefficient of carbon composites can be negative and close to zero; transverse expansion and conductivity are matrix-controlled. The book analyzes thermal stresses in laminates and structures (rings, tubes) with numerical examples.

Moisture

  • Water absorption by Fickian diffusion, mainly in the matrix; equilibrium moisture depends on ambient humidity.
  • Lower Tg and matrix-controlled properties; swelling and hygroscopic stresses.
  • Interface degradation and, in glass fibers, loss of fiber strength under stress.
ε_total = ε_mechanical + α·ΔT + β·ΔC

Combined effect

The combination of high temperature and moisture (hot-wet) is the worst case for compressive and shear strength. The book recommends determining design properties over the full range of service temperature and humidity.

Key pointResidual thermal stresses are always present and increase at lower service temperatures; for structures exposed to cold or cryogenic temperatures, the matrix cracking they cause must be checked separately.
NABAK CompositePage 13 of 19
Advanced Mechanics of Composite Materials and Structures
Advanced Mechanics of Composite Materials and Structures

12Time-dependent behavior: creep, fatigue and impact

Viscoelasticity and creep

The polymer matrix has time-dependent behavior, so matrix-controlled properties (transverse and shear) and angle-ply layers undergo creep and stress relaxation. The book uses the Boltzmann–Volterra hereditary theory:

ε(t) = σ(t)/E + ∫₀ᵗ K(t − τ)·σ(τ) dτ

K is the creep kernel, determined from creep tests. Using the correspondence principle, elastic solutions (including micromechanics and laminate theory) are converted to viscoelastic problems. Creep is negligible along the fibers but significant in ±45 layers and in the transverse direction.

Long-term strength

Under constant load, a composite may fail after some time (creep rupture or stress corrosion in glass fibers). The strength-time curve is used to set the long-term allowable stress; for glass/epoxy, long-term strength is much lower than short-term strength.

Fatigue

  • Diffuse damage: matrix cracking, delamination and fiber breakage; gradual loss of stiffness.
  • Unidirectional carbon composites have excellent fatigue resistance; glass composites are more sensitive.
  • Angle plies and tension-compression loading reduce life.
  • Hysteretic heating at high frequencies.

Impact and damage tolerance

Low-velocity impact can cause internal delamination and matrix cracking that is not visible from the surface but greatly reduces compressive strength. The book analyzes impact with contact models and the dynamic response of plates and shells, and examines the role of matrix toughness, outer ±45 plies and fabric structures in damage tolerance.

Durability

A combination of load, time, temperature, moisture and damage; the book stresses that durability must be confirmed by long-term tests under service-like conditions.

Key pointFor permanent loads, set allowable stress from long-term (not short-term) strength; this is vital for glass fiber FRP pipes, tanks and structures.
NABAK CompositePage 14 of 19
Advanced Mechanics of Composite Materials and Structures
Advanced Mechanics of Composite Materials and Structures

13Effects of the manufacturing process

One of the book's special chapters: composite properties are formed in the structure itself and during manufacture. The book shows that the same materials produce different properties with different processes.

Filament winding and fiber tension

  • Winding tension compacts the underlying layers and squeezes out excess resin; fiber volume fraction varies through the thickness.
  • As later layers are wound, tension in the underlying layers decreases (inner fibers may even go slack and wavy).
  • The book presents a model for calculating the tension distribution through the thickness and shows that variable (programmed) tension or staged curing improves uniformity.

Residual stresses

Chemical shrinkage of the resin, differences in thermal expansion coefficients and anisotropy create residual stresses. In thick filament-wound rings and cylinders, residual radial tensile stress can lead to circumferential cracks and delamination. The book presents methods for measuring (ring slitting and deformation measurement) and calculating these stresses.

Fiber waviness and porosity

  • Fiber waviness and misalignment: reduce stiffness and especially compressive strength; even a few degrees of deviation has a noticeable effect.
  • Porosity: severely reduces matrix-controlled properties (interlaminar shear, compression, transverse); each percent of voids cuts interlaminar shear strength by several percent.
  • Incomplete cure: lower Tg and environmental resistance.

Scale effects and test specimens

The properties of small flat specimens may differ from those of the real structure (for example a filament-wound pipe or tank). The book recommends determining design properties as far as possible on specimens with the same process and geometry as the structure (for example filament-wound rings and tubes).

Note for FRP productionIn pultrusion, uniform roving tension, control of fiber waviness in preforming, full cure and low void content are the same process factors the book lists for filament winding, and they directly affect the compressive and shear strength of profiles.
Key pointIn composites, the "material" is a product of the process; design properties must come from specimens made by the same process, and process control (fiber tension, voids, cure) is part of design.
NABAK CompositePage 15 of 19
Advanced Mechanics of Composite Materials and Structures
Advanced Mechanics of Composite Materials and Structures

14Optimal structures and pressure vessels

The optimal fibrous structure

The book defines the optimal structure as one in which all fibers lie along the principal stress lines and reach their strength simultaneously (uniform strength). With the monotropic model, for a laminate of ±φ layers under N_x and N_y:

N_x = h·σ̄₁·cos²φ    N_y = h·σ̄₁·sin²φ    ⇒   tan²φ = N_y/N_x,   h = (N_x + N_y)/σ̄₁

The second relation shows that the optimal thickness depends only on the sum of the loads, and a uniform-strength laminate has the lowest possible weight.

Cylindrical pressure vessel

N_x = pR/2, N_y = pR    ⇒   tan²φ = 2,   φ ≈ 54.7°

For a closed-end cylinder, an angle of 54.7 degrees brings the fibers to their strength limit in both directions simultaneously. In practice, a combination of hoop (90°) layers and low-angle helical layers is also common to suit the dome geometry.

Isotensoid domes and geodesic winding

In the end domes, the fiber angle varies with radius. Geodesic winding follows Clairaut's relation:

r·sinφ = r₀ = const

r₀ is the polar opening radius. The dome shape in which geodesic fibers carry load at uniform stress (isotensoid) is found by solving the membrane equilibrium equations together with this relation. The book describes the method of designing the dome shape and variable thickness (due to fiber build-up near the opening).

Other optimal structures

Uniform-strength rotating disks (fibers along special paths), tubes under combined loads and shells of revolution. Also composite vessels with metal or polymer liners (types III and IV), in which the liner provides sealing and the composite carries the load.

Key pointFilament-wound structures (pipes, tanks) are the best example of an "optimal fibrous structure"; with the correct winding angle and an isotensoid dome shape, composite pressure vessels achieve a specific strength several times that of steel.
NABAK CompositePage 16 of 19
Advanced Mechanics of Composite Materials and Structures
Advanced Mechanics of Composite Materials and Structures

15Anisogrid lattice structures

One of the book's most outstanding sections, based on the authors' practical experience in the space industry: composite lattice (anisogrid) shells made of unidirectional helical and hoop ribs.

Concept

  • The ribs are made of continuous unidirectional fiber (usually carbon) by automated filament winding into the grooves of a mandrel.
  • Each rib carries load only along its own axis (the fiber direction); the matrix carries almost no load.
  • Where ribs cross, fibers lie on top of each other and form a continuous joint.
  • There may be no outer skin, or only one for covering.

Design

Design variables: helical rib angle, and spacing and cross-section dimensions of the helical and hoop ribs. Constraints:

Failure modeDescription
Rib strengthRib stress below the compressive or tensile strength of the unidirectional ply
Local rib bucklingBuckling of the rib between nodes like a column
Global shell bucklingBuckling of the lattice cylinder with equivalent stiffness

The book gives analytical relations for the equivalent stiffness and these three modes and shows that in an optimal design all three are active simultaneously. The optimization equations give the rib angles and dimensions for minimum mass under axial compression and bending.

Advantages and applications

Composite lattice structures have been used in space adapters, launcher interstages and satellite bodies, and offer significant weight savings over stiffened or sandwich structures, good damage tolerance (damage to one rib is not transferred to others) and low-cost automated manufacture.

Key pointThe anisogrid lattice structure is the culmination of the book's philosophy: a material that is strong only along its fibers is used in a structure that loads it only in that direction. The result is the highest possible fiber efficiency.
NABAK CompositePage 17 of 19
Advanced Mechanics of Composite Materials and Structures
Advanced Mechanics of Composite Materials and Structures

16Conclusions and frequently asked questions

The book's ten golden points

  1. The advantage of composites lies only along the fibers; align the fibers with the load path.
  2. Take ply properties from tests; micromechanics is a tool for understanding.
  3. Ply transverse and shear strengths are tens of times lower than longitudinal strength.
  4. ±φ layers at intermediate angles behave nonlinearly and depend on the matrix.
  5. Quasi-homogeneous laminates (thin repeated plies) simplify analysis and eliminate couplings.
  6. The monotropic model is accurate and simple for the ultimate strength of optimal fibrous structures.
  7. Failure criterion: maximum stress for the fibers and a quadratic criterion for the matrix.
  8. The definition of failure (matrix cracking or fiber failure) determines the allowable stress.
  9. The manufacturing process (fiber tension, residual stress, voids, waviness) is part of design.
  10. Optimal structures (isotensoid vessels, anisogrid lattices) with uniform fiber strength have the lowest weight.

Applications for FRP manufacturers

For pultruded profiles: longitudinal fibers for axial and bending loads and mat and stitched layers for shear and transverse properties; process quality control for compressive strength. For filament-wound pipes and tanks: optimal winding angle, dome design and control of fiber tension and residual stresses. For all products: design with long-term strength and environmental conditions.

Frequently asked questions

What is the monotropic (netting) model? A model that assumes only the fibers carry load, along their own direction; it is used for preliminary design of filament-wound structures and for finding the optimal angle.

What is an anisogrid lattice structure? A shell of filament-wound unidirectional helical and hoop ribs with very high strength- and stiffness-to-weight ratios, for space structures.

Why do ±45 layers behave nonlinearly? Because load is carried mainly by shear in the matrix, which behaves nonlinearly and time-dependently; at large strains the fibers also rotate.

What is the optimal angle for a cylindrical pressure vessel? About 54.7 degrees, from tan²φ = 2.

NABAK CompositePage 18 of 19
Advanced Mechanics of Composite Materials and Structures
Advanced Mechanics of Composite Materials and Structures

17Glossary

English termMeaningShort explanation
Specific strength / stiffnessSpecific strength / stiffnessDivided by density
Unidirectional plyUnidirectional plyParallel fibers in a matrix
Angle-ply layerAngle-ply layerSymmetric ±φ
Fabric layerFabric layersWoven fibers with crimp
Lattice layerLattice layerUnidirectional ribs
Spatially reinforced compositeSpatially reinforced composite3D fibers
Quasi-homogeneous laminateThe quasi-homogeneous laminateThin repeated plies
Quasi-isotropic laminateThe quasi-isotropic laminateDirection-independent stiffness
Monotropic (netting) modelMonotropic (netting) modelOnly fibers carry load
MicrobucklingMicrobucklingFiber compressive failure
Hybrid compositeHybrid compositeSeveral fiber types
First-ply / ultimate failureFirst-ply / ultimate failureProgressive failure
Allowable stressAllowable stressDesign stress
Hereditary (Boltzmann–Volterra) theoryHereditary theoryViscoelasticity
Long-term strengthLong-term strengthCreep rupture
Winding tensionWinding tensionFiber tension in filament winding
Residual stressesResidual stressesProcess-induced
Fibre wavinessFiber wavinessLower compressive strength
Uniform-strength laminateUniform-strength laminateOptimal structure
Geodesic winding / ClairautGeodesic winding / Clairaut's relationr·sinφ = const
IsotensoidIsotensoidDome with uniform fiber stress
Anisogrid lattice structureAnisogrid lattice structureComposite lattice shell

Related keywords: advanced composite mechanics, composite structures, FRP composites, angle-ply layers, laminates, failure criteria, composite pressure vessels, filament winding, anisogrid lattice structures, composite creep and fatigue, optimal design, FRP profiles, NABAK Composite.

NABAK CompositePage 19 of 19