Fire Behavior of FRP Composites
Fire Properties of Polymer Composite Materials

Fire Properties of Polymer Composite Materials

Fire Behavior of FRP Polymer Composites: A Comprehensive Book Summary

A fire safety guide for FRP composites: thermal decomposition of resins, flammability, heat release rate, flame spread, smoke and toxicity, fire resistance, strength loss in fire, post-fire properties, flame retardants, protective coatings and fire standards

Authors of the original book: A. P. Mouritz, A. G. Gibson
Publisher: Springer — field: fire safety and thermo-mechanical behavior of composites
Prepared for: NABAK Composite

Why is this book vital for the FRP industry?

Fire is one of the main obstacles to the wider use of FRP composites in buildings, rail and marine transport, oil platforms and aerospace. The polymer matrix is organic and at high temperature decomposes, releases heat and smoke, and loses its stiffness and strength. Mouritz and Gibson's book is one of the first and most comprehensive references to examine both "fire reaction" (the material's contribution to fire growth) and "fire resistance" (structural performance during and after fire) with experimental data, thermo-mechanical models and fire-retardant solutions.

How to use this summary

  • Orange "Key point" boxes give the most important practical conclusion of each chapter for designing fire-retardant, safe products.
  • Gold "Note" boxes show how the material applies to producing FRP profiles, grating, panels and pipes.
  • The figures given are typical ranges from the literature and depend on formulation, thickness, heat flux and test method; for regulatory compliance, always rely on standard tests of your own product.
NABAK CompositePage 1 of 19
Fire Behavior of FRP Composites
Fire Properties of Polymer Composite Materials

Table of Contents

  1. 1Introduction: fire hazard in FRP composites
  2. 2Thermal decomposition of resins and composites
  3. 3Fire reaction: ignition and oxygen index
  4. 4Heat release rate and the cone calorimeter
  5. 5Flame spread, smoke and toxic gases
  6. 6Comparing the fire behavior of resins and fibers
  7. 7Thermal modeling of composites in fire
  8. 8Fire resistance: insulation and flame penetration
  9. 9Mechanical properties at high temperature
  10. 10Structural behavior and failure modeling in fire
  11. 11Post-fire mechanical properties
  12. 12Flame retardants and fire-retardant resins
  13. 13Coatings, insulation and protection strategies
  14. 14Health hazards in composite fires
  15. 15Fire regulations and standards
  16. 16Conclusions, application to FRP profiles and frequently asked questions
  17. 17Glossary of composite fire terms
The book's main message in one sentenceFire safety of FRP composites has two separate dimensions that must both be designed for: reducing the material's contribution to fire growth (later ignition, less heat, smoke and toxicity) and maintaining structural performance in fire (insulation, preventing flame penetration and carrying load); improving one does not necessarily improve the other.
NABAK CompositePage 2 of 19
Fire Behavior of FRP Composites
Fire Properties of Polymer Composite Materials

1Introduction: fire hazard in FRP composites

Fiber-reinforced polymer (FRP) composites have major advantages: light weight, corrosion resistance, insulation and durability. But the polymer matrix (polyester, vinyl ester, epoxy, etc.) is an organic, combustible material. In fire, the resin decomposes and releases flammable gases, smoke and toxic gases. As a result, the composite may both contribute to fire growth and the composite structure may weaken or collapse.

The book's two main concepts

ConceptDefinitionIndicators
Fire reaction (Fire reaction)How the material contributes to fire initiation and growth; important in the early stages of fire before flashoverTime to ignition, heat release rate, flame spread, oxygen index, smoke, toxic gases
Fire resistance (Fire resistance)The ability of a structural component to confine fire to a space and maintain stability; important in fully developed fireThermal insulation, preventing flame passage, load-bearing, time to failure

Stages of a compartment fire

  1. Ignition: a small source; time to ignition and surface flammability matter.
  2. Growth: flame spread and heat release from surfaces raise room temperature.
  3. Flashover: simultaneous ignition of all combustible surfaces; temperature about 600 °C and above.
  4. Fully developed fire: 900 to 1200 °C; structural resistance and compartmentation matter.
  5. Decay: as fuel runs out.

Incidents and applications

The book refers to incidents in aircraft, trains, ships and offshore platforms in which smoke and toxic gases caused more casualties than flames. These experiences led to strict regulations for composite materials in these industries. Sensitive applications: aircraft cabin interiors, trains and metros, ship hulls and superstructures, grating and pipes on oil platforms, and FRP panels and profiles in buildings and tunnels.

Key pointIn most fires, smoke and toxic gases (especially carbon monoxide) cause most casualties, not flames. Choosing composites for enclosed spaces and escape routes must also be based on smoke and toxicity, not just time to ignition.
NABAK CompositePage 3 of 19
Fire Behavior of FRP Composites
Fire Properties of Polymer Composite Materials

2Thermal decomposition of resins and composites

When an FRP composite is heated, the following processes occur in order of temperature: softening of the resin at the glass transition temperature (Tg), evaporation of moisture and volatiles, thermal decomposition (pyrolysis) of the polymer chains producing flammable gases, char formation in some resins, and at very high temperatures char oxidation and fiber damage.

Polymer decomposition mechanisms

  • Random chain scission: producing smaller fragments and volatiles.
  • Depolymerization: as in PMMA; abundant fuel and little char.
  • Side-group elimination: such as release of styrene from polyester and vinyl ester or HCl from PVC.
  • Crosslinking and charring: as in phenolics and some aromatic thermoplastics; the char forms an insulating layer.

Thermogravimetric analysis (TGA)

TGA measures mass loss as a function of temperature. Important outputs: onset temperature of decomposition, temperature of maximum mass loss rate, number of decomposition stages and char yield (percentage of residual mass). High char yield is usually associated with lower heat release and better fire behavior.

ResinMain decomposition range (°C)Char yieldNote
Polyester~300–400Very low (less than about 10%)Styrene release; heavy smoke
Vinyl ester~350–450LowSimilar to polyester, slightly more stable
Epoxy~350–450Low to mediumDepends on the hardener; amines produce HCN gas
PhenolicAbout 400–600 (multi-stage)High (about 50% or more)Stable char; low smoke and heat
Advanced thermoplastics (PEEK, PPS)~500–600Medium to highExcellent thermal stability

Indicative ranges; values depend on formulation and heating rate.

Decomposition kinetics

∂ρ/∂t = −A·ρ₀·[(ρ − ρ_f)/ρ₀]ⁿ·exp(−E/RT)

ρ is the instantaneous density, ρ₀ the initial and ρ_f the final density (char and fibers). A, E and n are obtained from TGA tests at several heating rates and are inputs to the thermal models in chapter 7. Decomposition is endothermic and absorbs part of the heat.

Fiber behavior

Glass fibers do not burn but soften and melt at about 700 to 900 °C, and their strength falls from about 250 to 300 °C onward. Carbon fibers oxidize and thin in air from about 450 to 500 °C. Aramid fibers are organic and decompose.

Key pointChar yield is the most important chemical indicator of a resin's fire behavior: more char means less gaseous fuel, a protective insulating layer, and less heat and smoke. That is why phenolic resin is the first choice for fire-retardant applications.
NABAK CompositePage 4 of 19
Fire Behavior of FRP Composites
Fire Properties of Polymer Composite Materials

3Fire reaction: ignition and oxygen index

Time to ignition

Ignition occurs when the composite surface reaches a temperature at which the flux of decomposition gases is enough to form a flammable mixture. For a "thermally thick" material:

t_ig = (π/4)·k·ρ·c·[(T_ig − T₀) / q̇″]²     ⇒   1/√t_ig ∝ q̇″

Plotting 1/√t_ig against radiant heat flux gives the critical heat flux (the lowest flux that causes ignition) and the "thermal response parameter". k·ρ·c is the material's thermal inertia; the larger it is, the more slowly the surface heats and ignites.

Factors affecting time to ignition

  • Resin type: phenolics and advanced thermoplastics ignite later.
  • Fiber volume fraction: more fiber means less fuel and more thermal inertia; later ignition.
  • Surface layer: a gel coat or resin-rich veil may ignite earlier; protective coatings delay ignition.
  • Thickness: thin parts (thermally thin) reach ignition temperature sooner.
  • Heat flux: time to ignition falls rapidly as flux increases.

Limiting oxygen index (LOI)

The minimum percentage of oxygen in an oxygen-nitrogen mixture needed to sustain flaming of a vertical specimen ignited from the top (ASTM D2863, ISO 4589). Air contains about 21% oxygen; materials with an LOI above about 26 to 28 are usually considered "self-extinguishing" in air.

Composite (glass fiber)Approximate LOI (%)
Standard polyester~20–28
Fire-retardant polyester or vinyl ester (halogenated or ATH)About 30–50 and higher
Epoxy~25–35
PhenolicAbout 40–60 and higher

UL 94 test

A small-flame test on a horizontal or vertical specimen; ratings HB, V-2, V-1 and V-0 based on extinguishing time and flaming drips. V-0 is the best vertical rating.

NoteThe book stresses that LOI and UL 94 are "small-scale, small-flame" tests and do not predict behavior in a real fire (high heat flux); they are useful for comparing formulations, not for proving safety.
Key pointLonger time to ignition means more time for escape and firefighting. Increasing fiber volume fraction, removing resin-rich surface layers and using a resin with higher thermal stability are the simplest ways to improve the ignitability of FRP composites.
NABAK CompositePage 5 of 19
Fire Behavior of FRP Composites
Fire Properties of Polymer Composite Materials

4Heat release rate and the cone calorimeter

The book considers heat release rate (HRR) the most important fire reaction indicator, because it directly determines how fast a fire grows and whether it reaches flashover.

Cone calorimeter (ISO 5660, ASTM E1354)

A horizontal 100×100 mm specimen is placed under a conical heater with a given radiant flux (usually 25, 50 or 75 kW/m²). Heat release is measured by the oxygen consumption principle: for most organic materials, about 13.1 MJ of heat is released per kilogram of oxygen consumed.

OutputMeaning
t_igTime to ignition
pHRR (peak heat release rate)Fire intensity; the most important hazard indicator
Average HRR (e.g. 180 or 300 seconds)Sustained heat release
THR (total heat released)Total available fuel
MLR (mass loss rate)Rate of decomposition
EHC (effective heat of combustion)Heat per mass of gas burned
SEA and CO and CO₂ productionSmoke and gases

Shape of the HRR curve in composites

In a thick char-forming composite, HRR peaks quickly after ignition and then falls as a char and fiber insulating layer forms at the surface (the char layer keeps heat away from the underlying resin). In a thin composite, two peaks may appear (back-face heating and final decomposition). In a non-charring composite such as polyester, the peak is higher and broader.

Combined fire hazard indices

Flashover propensity ≈ pHRR / t_ig     FIGRA = max(HRR(t)/t)

The Petrella plot (pHRR/t_ig against THR) is a simple way to rank materials: materials low on both indices have lower fire hazard. The book compares data for dozens of composite systems this way.

Factors affecting HRR

  • Resin type: phenolics and aromatic thermoplastics lowest; polyester and vinyl ester highest.
  • Fiber volume fraction: less resin means less fuel and lower HRR.
  • Heat flux: pHRR increases roughly linearly with flux.
  • Flame retardants and coatings: substantial reduction in pHRR.
Key pointpHRR is the most important cone calorimeter number for FRP composites; reducing it lowers fire growth and the likelihood of flashover. Always state and compare the test heat flux and specimen thickness in reports.
NABAK CompositePage 6 of 19
Fire Behavior of FRP Composites
Fire Properties of Polymer Composite Materials

5Flame spread, smoke and toxic gases

Flame spread

The rate at which flame advances over a surface determines how quickly fire reaches other surfaces. Upward flame spread (in the direction of hot gas flow) is much faster than downward or lateral spread. Common tests:

  • ASTM E84 (Steiner tunnel): flame spread index (FSI) and smoke developed index (SDI); common in US buildings. Class A means an FSI of at most 25.
  • ISO 5658-2 and IMO LIFT: lateral flame spread; for ships.
  • BS 476 Part 7: surface spread of flame; classes 1 to 4.
  • SBI (EN 13823): single burning item test in a corner for the European Euroclass classification.

Smoke

Smoke reduces visibility and makes escape difficult. Measures: specific optical density (Ds) in the NBS smoke chamber (ASTM E662, ISO 5659-2) and specific extinction area (SEA) in the cone calorimeter.

  • Resins containing aromatic rings and styrene (polyester and vinyl ester) produce dense black smoke.
  • Phenolic produces very little smoke; that is why it is preferred in aircraft interiors, metros and tunnels.
  • Halogenated flame retardants increase smoke; ATH reduces it.

Toxic gases

GasSourceEffect
CO (carbon monoxide)All resins; more in incomplete combustion and after flashoverThe main cause of death; binds to hemoglobin
HCN (hydrogen cyanide)Nitrogen-containing resins (epoxy with amine hardener, polyurethane, aramid)Highly toxic; cellular asphyxiation
HCl and HBrHalogenated flame retardants, PVCIrritant and corrosive; damages equipment
CO₂All materialsIncreases breathing rate and uptake of other toxicants
Aldehydes, benzene, styreneResin decompositionIrritation and toxicity

Toxicity is assessed with the fractional effective dose (FED) approach: the contribution of each gas relative to its lethal concentration is summed. Low oxygen also has a toxic effect.

Key pointHalogenated flame retardants may reduce flame but increase smoke and toxic, corrosive gases; in enclosed spaces, halogen-free systems (phenolic, ATH, phosphorus) are a safer choice.
NABAK CompositePage 7 of 19
Fire Behavior of FRP Composites
Fire Properties of Polymer Composite Materials

6Comparing the fire behavior of resins and fibers

The book compiles and compares extensive cone calorimeter and other test data for common composite systems. The table below summarizes the qualitative trends (for glass fiber at moderate heat flux):

ResinTime to ignitionpHRRSmokeFire-retardant use
Ortho/iso polyesterShortHighHighOnly with fire-retardant additives
Vinyl esterShort to mediumHighHighBrominated grade or with additives
EpoxyMediumModerate to highMedium to highPhosphorus-containing or brominated grade
PhenolicLongLowVery lowExcellent; inherently fire-retardant
Bismaleimide and cyanate esterLongLow to moderateLow to mediumAerospace
PEEK, PPS, PEIVery longVery lowLowAerospace; expensive

Effect of fibers

  • Glass: non-combustible; reduces heat and smoke by lowering the resin share; after the surface resin burns away, glass plies form a physical barrier.
  • Carbon: higher thermal conductivity (heat reaches the interior faster) but stable at moderate temperatures; oxidizes at high temperature.
  • Aramid: decomposes itself and adds to the fuel; produces HCN.
  • Natural fibers: combustible and increase fire hazard.

Effect of construction

A sandwich with a polymer foam or balsa core adds a lot of fuel to the fire if the fire breaks through the skin, and the foam core may melt or decompose. Thicker skins and non-combustible cores (such as phenolic foam or mineral cores) reduce this risk.

Note for FRP profilesPultruded profiles have high fiber volume fractions (and therefore less fuel), which helps their fire behavior. For demanding applications (tunnels, metros, oil platforms), pultruded profiles and grating with phenolic resin are common, and for general building applications, polyester or vinyl ester containing ATH with surface veil.
Key pointResin choice has the greatest effect on a composite's fire behavior; glass fibers help by reducing fuel but are no substitute for a fire-retardant resin.
NABAK CompositePage 8 of 19
Fire Behavior of FRP Composites
Fire Properties of Polymer Composite Materials

7Thermal modeling of composites in fire

To predict how a composite structure behaves in fire, the temperature distribution through the thickness over time must first be known. The book describes one-dimensional thermo-chemical models, mainly based on the work of Henderson and co-workers, and compares them with experiments.

Governing equation (Henderson model)

ρ·Cp·∂T/∂t = ∂/∂x(k·∂T/∂x) − ṁ_g·Cp,g·∂T/∂x − (∂ρ/∂t)·(Q_p + h_c − h_g)
  • First term: heat conduction through the thickness.
  • Second term: heat carried by decomposition gases as they flow through the char toward the hot surface (cooling).
  • Third term: the endothermic heat of decomposition (Q_p), which absorbs heat.

This equation is coupled with the decomposition kinetics equation (Arrhenius) and gas mass conservation. The properties k, Cp and ρ are interpolated between virgin and charred material according to the degree of decomposition.

Boundary conditions

  • Fire-exposed surface: radiant and convective heat flux; or a standard fire time-temperature curve.
  • Back surface: convection and radiation to the surroundings or insulation.

Zone structure through the thickness

ZoneCondition
Char and fibers (fire surface)Resin decomposed; porous insulating layer
Decomposition frontActive pyrolysis; gas generation
Softened zoneTemperature above Tg but no decomposition; reduced strength
Virgin material (cold side)Nearly full properties

Validation

The model has been compared with thermocouples embedded through the thickness of specimens under constant flux or standard fire and shows good accuracy. The book notes that moisture evaporation (a temperature plateau at about 100 °C), delamination, char cracking and thickness changes can reduce accuracy. To predict HRR, the thermal model is combined with the mass fraction of gas burned and the heat of combustion.

Key pointA thick composite is "self-insulating": the char and fiber layer, low conductivity, endothermic decomposition and gas cooling keep the cold-side temperature low for a long time; this advantage is very valuable in walls and partition panels.
NABAK CompositePage 9 of 19
Fire Behavior of FRP Composites
Fire Properties of Polymer Composite Materials

8Fire resistance: insulation and flame penetration

Fire resistance is measured in furnace tests with standard time-temperature curves and is usually expressed by three criteria:

CriterionDefinition
Integrity (E)No passage of flame and hot gases through cracks or holes
Insulation (I)Back-face temperature rise of at most about 140 °C (average) or 180 °C (point)
Load-bearing (R)Sustaining load without collapse or excessive deformation

Standard fire curves

ISO 834 (cellulosic): T = 20 + 345·log₁₀(8t + 1)    (t in minutes)
  • Cellulosic (ISO 834, ASTM E119): building fire; about 945 °C at 60 minutes.
  • Hydrocarbon (UL 1709, EN 1363-2): very rapid growth to about 1100 °C in a few minutes; for the oil and gas industry.
  • Jet fire: very high heat flux and mechanical erosion; offshore platforms.
  • Pool and tunnel fire (RWS): up to about 1350 °C for tunnels.

Composite behavior in furnace tests

  • Because of their low thermal conductivity, composites are much better than metals for "insulation"; the back face of a steel wall heats up quickly.
  • The time for the back face to reach the critical temperature increases roughly with thickness; phenolic composites perform better thanks to their stable char.
  • For "integrity", complete burn-off of the resin and delamination can create a path for flame; sandwich structures with polymer cores are more vulnerable.
  • For "load-bearing", composites are weakest because the resin softens at a low temperature (Tg) (chapters 9 and 10).
NoteThe book shows that suitable composite panels (phenolic, thick or insulated) can meet the demanding fire resistance ratings of the marine and offshore industries, provided they are properly protected and the details are well designed.
Key pointFRP composites outperform metals in "insulation" and are weaker in "load-bearing". Fire resistance design must secure load-bearing through insulation, thickness or lower working stress.
NABAK CompositePage 10 of 19
Fire Behavior of FRP Composites
Fire Properties of Polymer Composite Materials

9Mechanical properties at high temperature

The structural behavior of a composite in fire starts with the behavior of the matrix at high temperature. As the temperature approaches the resin's Tg (about 80 to 150 °C for most pultrusion and lay-up resins), the matrix modulus drops several-fold; this temperature is far below the decomposition temperature.

Matrix- and fiber-controlled properties

PropertyControlled byBehavior at high temperature
Longitudinal tensile strength and modulusFibersRelatively well retained up to high temperatures; slow loss
Compressive strengthMatrix (lateral support of fibers)Sharp loss near Tg; microbuckling
Shear and interlaminar strengthMatrix and interfaceSharp loss near Tg
Flexural modulusCombinationSignificant loss

Empirical temperature-dependence model

P(T) = (P_U + P_R)/2 − (P_U − P_R)/2 · tanh[ k·(T − T_k) ]

P_U is the room-temperature property, P_R the residual property at high temperature (after the glass transition), T_k the mid-point temperature of the loss (near Tg) and k a slope parameter. This simple relation fits modulus and strength data well through the glass transition and is the basis of structural fire models.

Time-dependent effects

  • Creep: at temperatures near Tg, creep is rapid and substantial; time to failure under constant load becomes short.
  • Moisture: lowers Tg and shifts the loss to lower temperatures.
  • Post-cure in fire: with slow heating, additional cure may raise Tg slightly.

Fibers at high temperature

The strength of glass fibers falls from about 200 to 300 °C and stays permanently lower after heating and cooling; carbon is stable up to its oxidation temperature.

Key pointFor composites in fire, the critical structural temperature is the resin's Tg, not the ignition or decomposition temperature. Choosing a high-Tg resin (such as properly cured vinyl ester or epoxy, or phenolic) increases load-bearing time in fire.
NABAK CompositePage 11 of 19
Fire Behavior of FRP Composites
Fire Properties of Polymer Composite Materials

10Structural behavior and failure modeling in fire

The book presents a "thermo-mechanical" approach for predicting the time to failure of a composite structure under simultaneous load and fire; a section that results from the authors' extensive research.

Model steps

  1. Thermal model: the temperature distribution through the thickness at each instant (chapter 7).
  2. Dividing the thickness into thin layers and assigning temperature-dependent properties (the tanh relation) to each layer.
  3. Calculating overall stiffness and strength by summing the layer contributions (as in laminate theory); charred layers contribute zero or negligibly.
  4. Comparison with the applied load: failure occurs when the remaining capacity falls below the load.

Tension in fire

Because the fibers carry the load and fiber strength loss is slow, a composite under tension survives longer in fire. Failure occurs through gradual reduction of the effective section and strength loss of the hot fibers.

Compression in fire

Composites are far more vulnerable under compression: as the surface layers heat above Tg, the matrix no longer supports the fibers and the compressive capacity of those layers becomes almost zero. In addition, the loss of bending stiffness and eccentricity (a stiffness gradient through the thickness that shifts the stiffness centroid toward the cold side) accelerate global buckling. Time to failure in compression may be several times shorter than in tension.

FactorEffect on time to failure
Stress level (ratio of load to capacity)Higher load, much shorter time to failure
Heat fluxHigher flux, faster heating and failure
ThicknessGreater thickness, longer time (cold margin)
Load typeTension longest; compression and shear shortest
Resin TgHigher Tg, longer time

Sandwich structures

In sandwiches, softening of the polymer foam core and the skin-core adhesive at low temperature causes wrinkling of the compressive skin and loss of composite action. Balsa or phenolic cores behave better.

Key pointComposite compression members (columns, compression flanges of beams, decks) are the most critical in fire. Safe fire design for them usually requires insulation or a lower stress level.
NABAK CompositePage 12 of 19
Fire Behavior of FRP Composites
Fire Properties of Polymer Composite Materials

11Post-fire mechanical properties

After a fire, it must be decided whether the composite structure is safe, should be repaired or must be replaced. For this assessment, the book provides experimental data and a simple, practical "two-layer" model.

Two-layer model

After fire, the composite section is divided into two zones: a charred, damaged layer (fire side) with almost zero strength and an intact layer (cold side) with nearly original properties. The boundary between them is set by the depth of the resin's critical decomposition temperature.

σ_post ≈ σ₀·(1 − d_c/d)    (tension, compression)     E_post·I_post from the intact layer only (bending)

d is the total thickness and d_c the depth of the damaged layer. Char depth increases with the square root of exposure time and with heat flux. The model agrees well with tension, compression and flexure data for glass/polyester, vinyl ester and phenolic composites.

Main trends

  • Properties decrease continuously with increasing fire exposure time and heat flux.
  • Matrix-controlled properties (compression, shear, flexure) drop faster than tension.
  • Glass fiber damage (permanent strength loss after heating above about 300 °C) can be present even in the apparently intact zone.
  • Phenolic char is more effective at protecting the underlying layer but has no strength itself.

Post-fire non-destructive assessment

Visual inspection, tap testing, ultrasonics and thermography to detect delamination and damage depth; Barcol hardness measurement and DSC on surface samples to detect thermal damage to the resin below its decomposition temperature.

Key pointAn intact-looking back face is no sign of structural soundness; delamination and resin softening may have occurred in depth. Post-fire assessment should determine the damage depth and calculate the remaining capacity (two-layer model).
NABAK CompositePage 13 of 19
Fire Behavior of FRP Composites
Fire Properties of Polymer Composite Materials

12Flame retardants and fire-retardant resins

Flame retardants improve the fire behavior of FRP composites through one or more mechanisms: gas phase (quenching flame radicals or diluting gases) or condensed phase (increasing char, cooling, forming a barrier).

Flame retardantMechanismAdvantagesDrawbacks
Alumina trihydrate (ATH)Endothermic decomposition from about 200 °C; releases water vapor; dilution and an oxide layerCheap, halogen-free, reduces smokeHigh loadings needed; high viscosity and loss of mechanical properties
Magnesium hydroxide (MDH)Similar to ATH, from about 300 °CHigher processing stabilityHigh loadings needed
Halogenated (bromine, chlorine) + antimonyQuenching radicals in the flameEffective at low loadingsSmoke and toxic, corrosive gases; environmental restrictions
Phosphorus-based (organic and inorganic)Increases char in the condensed phase; gas-phase effectHalogen-free; effective in epoxyMay reduce Tg or properties
IntumescentSwelling and formation of a thick insulating charExcellent thermal protectionUsually as a coating; sensitive to moisture
Nanoparticles (nanoclay, nanotubes)Forming a surface barrier layerReduces pHRR at low loadingsLittle effect on time to ignition; difficult dispersion

Inherently fire-retardant resins

  • Phenolic: the best combination of time to ignition, HRR, smoke and toxicity; but more brittle, with condensation cure releasing water and creating voids.
  • Brominated polyester and vinyl ester: effective fire retardancy with the drawbacks of halogens.
  • Phosphorus-containing epoxy, cyanate ester, bismaleimide and advanced thermoplastics for aerospace applications.

Balancing processing and properties

Adding mineral fillers at tens of weight percent raises viscosity, makes fiber impregnation difficult and reduces mechanical properties (especially shear and impact). In pultrusion, ATH formulation must be matched with the release agent, die temperature and pull speed.

Key pointNo flame retardant improves all indicators; halogens reduce flame but increase smoke, and nanoparticles reduce pHRR but don't change time to ignition. The choice must be based on the requirements of the target standard (flame, heat, smoke or toxicity).
NABAK CompositePage 14 of 19
Fire Behavior of FRP Composites
Fire Properties of Polymer Composite Materials

13Coatings, insulation and protection strategies

Instead of changing the whole material, the fire-exposed surface can be protected. The book compares surface protection strategies in terms of effectiveness, weight and cost.

Protective coatings

  • Intumescent coatings: at about 200 to 300 °C they swell tens of times and form a thick insulating char; they delay ignition, reduce HRR and keep the underlying composite cool.
  • Ceramic and mineral coatings: a stable thermal barrier at very high temperatures; may crack or debond.
  • Fire-retardant gel coat and veil: a surface layer containing ATH or phosphorus; improves ignition and flame spread behavior.
  • Thin metal sheets or foil: reflect radiation and spread heat.

Insulation and fire barriers

  • Mineral or ceramic fiber blankets: in marine structures to achieve fire resistance ratings (e.g. 30 or 60 minutes).
  • Fire-resistant fabrics and silica layers at the laminate surface as a physical barrier.
  • Non-combustible cores in sandwiches (phenolic foam, mineral cores).

Design strategies

PurposeEffective approach
Delaying ignition and reducing flame spreadFire-retardant resin, fire-retardant surface layer, intumescent coating
Reducing smoke and toxicityPhenolic, ATH, avoiding halogens
Insulation and integrityGreater thickness, charring resin, mineral fiber insulation
Maintaining load-bearingHigh-Tg resin, insulation, lower working stress, fibers along the tension path

Practical considerations

Coatings add weight and cost and must withstand moisture, impact, UV and abrasion over the service life. Coating adhesion to the composite at high temperature and during swelling is vital. Protection must be continuous over the whole fire-exposed surface, including edges and joints.

Key pointCombining "a material with suitable fire behavior" and "surface protection" is usually more economical than adding a large amount of flame retardant to the whole material, and reduces mechanical properties less.
NABAK CompositePage 15 of 19
Fire Behavior of FRP Composites
Fire Properties of Polymer Composite Materials

14Health hazards in composite fires

Toxic gases and smoke

As noted in chapter 5, CO is the main cause of toxicity, and its concentration rises sharply after flashover and under oxygen-starved conditions. HCN is released from nitrogen-containing resins and hardeners, and acid gases from halogens. Besides causing death, toxicity and smoke make escape difficult by reducing visibility and irritating the eyes and respiratory tract.

Fiber release

  • Carbon fibers: oxidize and thin in fire and may reach respirable diameters (below about 3 micrometers); being conductive, airborne carbon particles can short-circuit electrical equipment.
  • Glass fibers: diameters are usually larger than the respirable limit, but fracture and partial melting may produce fine particles; skin and eye irritation.
  • Surface dust and soot: char and soot particles carrying toxic organic compounds.

Firefighter safety and post-fire clean-up

The book recommends that in incidents involving composites, especially carbon composites (such as aircraft crashes), firefighters and clean-up teams use full respiratory protection, protective clothing and fiber fixing methods (spraying adhesive or wax coatings on the debris) so that loose fibers do not become airborne.

Toxicity tests

MethodApplication
NBS smoke chamber with gas analysis (FTIR)Aircraft, trains, ships
Toxicity index (e.g. NF X 70-100, BS 6853, EN 45545-2)Rail
IMO FTP Code Part 2Smoke and toxicity of marine materials
FED method based on gas concentrationsHuman hazard assessment
Key pointFor FRP products used in occupied spaces and escape routes (metros, tunnels, ships, public buildings), smoke and toxicity must be considered from the start, when choosing the resin and flame retardant; fixing them later is difficult and costly.
NABAK CompositePage 16 of 19
Fire Behavior of FRP Composites
Fire Properties of Polymer Composite Materials

15Fire regulations and standards

The book reviews the fire regulations of each industry. The general message: requirements are set by the hazard and the possibility of escape; the harder escape is (aircraft, submarines, tunnels), the stricter the requirements. Some of the standards below were finalized or updated after the book was published; always check the latest edition.

IndustryExample regulations and testsFocus
AviationFAR 25.853 (vertical flame test, OSU heat release, smoke density), fire penetration testHeat release and smoke in the cabin
MarineSOLAS, IMO FTP Code, HSC Code (flame spread, smoke and toxicity, panel fire resistance tests)High-speed craft and composite structures
RailEN 45545 (Europe), BS 6853, NF F 16-101, NFPA 130Hazard levels and requirement levels by train type and installation location
BuildingEN 13501-1 (Euroclass A1 to F, with smoke classes s and droplet classes d), ASTM E84, BS 476Reaction to fire of building materials
Building fire resistanceEN 13501-2, ISO 834, ASTM E119 (R, E and I classes)Structural and separating elements
Offshore oil and gasHydrocarbon and jet fire tests, requirements for grating and pipe (e.g. ISO 14692 for GRP pipe)Maintaining integrity in severe fire
Electrical equipmentUL 94, IEC 60695Small flame and self-extinguishing

Practical notes

  • A test result is valid only for the same formulation, thickness, layup, coating and installation method; changing any of them may change the rating.
  • Small-scale tests (cone calorimeter) for product development; medium- and large-scale tests for certification.
  • No single measure fully describes fire behavior; each standard assesses a combination of indicators.
Note for FRP profile manufacturersTo enter the building, rail and oil and gas markets, obtaining Euroclass or ASTM E84 ratings and, where needed, EN 45545 for key products (grating, handrail, cable tray, building profiles), and keeping valid test reports, is an important competitive advantage.
Key pointBefore designing a fire-retardant formulation, determine the standard and target rating of the destination market; the requirements of different industries limit different indicators, and a formulation that is optimal for one may fail another.
NABAK CompositePage 17 of 19
Fire Behavior of FRP Composites
Fire Properties of Polymer Composite Materials

16Conclusions, application to FRP profiles and frequently asked questions

The book's ten golden points

  1. Reaction to fire and resistance to fire are two separate topics with different solutions.
  2. Smoke and CO, not flame, are the main cause of fire casualties.
  3. Resin char yield is the best chemical indicator of fire behavior; phenolic is the best.
  4. pHRR is the most important fire growth hazard indicator in the cone calorimeter.
  5. More fiber means less fuel, but it is no substitute for a fire-retardant resin.
  6. A thick composite is a good insulator and outperforms metal in "insulation".
  7. The critical structural temperature is Tg; compression members fail earlier than tension members.
  8. After fire, the two-layer model estimates remaining capacity from damage depth.
  9. Every flame retardant has pros and cons; halogens raise smoke and toxicity.
  10. Design for fire must start with the standard of the destination market.

Application to producing fire-retardant FRP profiles

For pultruded profiles and grating: choose the resin to suit the requirement (phenolic for low smoke and toxicity, vinyl ester or polyester with ATH or phosphorus compounds for general use), a high fiber volume fraction, fire-retardant surface veil, control of Tg through full cure, and verification with the target standard tests. In load-bearing applications exposed to fire, capacity must be calculated with high-temperature properties or protection must be provided.

Frequently asked questions

What is the difference between reaction to fire and resistance to fire? Reaction to fire is the material's contribution to fire growth (ignition, heat, flame spread, smoke and toxicity); resistance to fire is a structure's ability to maintain insulation, integrity and load-bearing during a fire.

Which resin is best for fire-retardant FRP profiles? Phenolic has the best behavior; polyester and vinyl ester become fire-retardant with additives such as ATH or phosphorus.

Why does compressive strength drop earlier in fire? Because it is matrix-controlled and drops rapidly near the resin's Tg, whereas tension is fiber-controlled.

Is FRP worse than steel in fire? In load-bearing and combustibility, yes; but in insulation and preventing heat transfer to adjacent spaces, a thick composite is much better than unprotected steel.

NABAK CompositePage 18 of 19
Fire Behavior of FRP Composites
Fire Properties of Polymer Composite Materials

17Glossary of composite fire terms

English termMeaningShort explanation
Fire reactionReaction to fireThe material's contribution to fire growth
Fire resistanceFire resistanceStructural performance in fire
Pyrolysis / Char yieldPyrolysis / char yieldThermal decomposition / residual mass
TGAThermogravimetryMass loss with temperature
Time to ignitionTime to ignitiont_ig
Critical heat fluxCritical heat fluxMinimum flux for ignition
LOILimiting oxygen indexMinimum oxygen for burning
Heat release rate (HRR / pHRR)Heat release rate / peakMain hazard indicator
Cone calorimeterCone calorimeterISO 5660
Oxygen consumptionOxygen consumption~13.1 MJ/kg O₂
FlashoverFlashoverSimultaneous ignition of the whole space
Flame spread indexFlame spread indexASTM E84
Specific optical density (Ds)Specific optical density of smokeNBS smoke chamber
FEDFractional effective doseToxicity assessment
Integrity / Insulation / Load-bearing (E/I/R)Integrity / insulation / load-bearingFire resistance criteria
Cellulosic / Hydrocarbon fire curveCellulosic / hydrocarbon fire curveISO 834 / UL 1709
Jet fireJet fireOil and gas industries
Two-layer modelTwo-layer modelPost-fire properties
Flame retardant (ATH, MDH)Flame retardantFlammability-reducing additive
Intumescent coatingIntumescent coatingSwelling coating
EuroclassEuropean classificationEN 13501-1
Phenolic resinPhenolic resinInherently fire-retardant resin

Related keywords: composite fire behavior, FRP composites in fire, fire resistance, fire-retardant, fire-retardant FRP profiles, phenolic resin, heat release rate, cone calorimeter, smoke and toxicity, ATH, intumescent coating, fire standards, NABAK Composite.