Mechanics of FRP Composite Materials
Principles of Composite Material Mechanics

Principles of Composite Material Mechanics

Principles of Composite Material Mechanics: A Comprehensive Book Summary

A scientific guide to designing and analyzing FRP composites: stress-strain behavior of the orthotropic lamina, micromechanics and the rule of mixtures, failure criteria, classical lamination theory and the ABD matrix, effects of moisture and temperature, viscoelasticity, fracture mechanics and mechanical testing

Author of the original book: Ronald F. Gibson
Publisher: CRC Press — field: solid mechanics and design of composite structures
Prepared for: NABAK Composite

Why is this book a foundation of composite mechanics?

This book is one of the most widely used textbooks on composite mechanics in universities worldwide. Its path is clear and logical: from fibers and matrix (micromechanics) to a single composite ply (lamina), from the ply to the multi-ply laminate, and from the laminate to beams, plates and structures. At each stage, stiffness and strength, environmental effects (temperature and moisture) and time-dependent behavior are all examined. For FRP profile producers and designers, this book is the knowledge behind technical property tables and structural calculations.

How to use this summary

  • Orange "Key point" boxes are the most important engineering conclusion of each chapter.
  • Gold "Note" boxes show how the material relates to designing and producing FRP composite products.
  • Notation follows the book's convention: direction 1 along the fibers, direction 2 perpendicular to the fibers in the plane and direction 3 through the thickness.
  • Example figures are for a sense of scale and are not a substitute for your material test data.
NABAK CompositePage 1 of 20
Mechanics of FRP Composite Materials
Principles of Composite Material Mechanics

Table of Contents

  1. 1Introduction: FRP composites and basic mechanics concepts
  2. 2Constituents: fibers, matrix and interface
  3. 3Anisotropy and material symmetry
  4. 4Stress-strain relations of the orthotropic lamina
  5. 5Axis transformation and off-axis behavior
  6. 6Micromechanics of stiffness: rule of mixtures and Halpin-Tsai
  7. 7Lamina strength and failure criteria
  8. 8Micromechanics of strength
  9. 9Thermal and moisture (hygrothermal) behavior
  10. 10Discontinuous fiber composites and nanocomposites
  11. 11Classical lamination theory and the ABD matrix
  12. 12Layup design and laminate strength
  13. 13Composite beams and plates: bending, buckling and vibration
  14. 14Viscoelasticity, creep and damping
  15. 15Fracture mechanics and delamination
  16. 16Mechanical testing of composites
  17. 17Conclusions, application to FRP profiles and frequently asked questions
  18. 18Glossary of composite mechanics terms
The book's main message in one sentenceFRP composite is a "designable" material: by choosing the fibers, volume fraction and ply angles, stiffness and strength can be placed exactly in the direction the structure needs; composite mechanics is the quantitative tool for this design.
NABAK CompositePage 2 of 20
Mechanics of FRP Composite Materials
Principles of Composite Material Mechanics

1Introduction: FRP composites and basic mechanics concepts

A composite material is a combination of two or more distinct materials that can be told apart at the macroscopic scale and together produce better properties than either alone. In fiber-reinforced polymer (FRP) composites, high-strength, high-stiffness fibers are placed in a polymer matrix. The matrix protects the fibers, transfers load between them and prevents them from buckling in compression.

Why composites? Specific strength and stiffness

The main advantage of composites lies in specific properties (divided by density). Very thin fibers have fewer flaws and therefore show much higher strength than the same material in bulk form (the size effect).

MaterialDensity (g/cm³)Modulus (GPa)Tensile strength (MPa)
Steel7.8200400–1500
Aluminum2.770300–550
Unidirectional glass/epoxy (Vf≈0.6)~2.0About 40–45 (longitudinal)About 1000 (longitudinal)
Unidirectional carbon/epoxy (Vf≈0.6)~1.6About 130–180 (longitudinal)About 1500–2200 (longitudinal)

Typical orders of magnitude; transverse values are far lower.

Basic concepts the book is built on

  • Heterogeneity: properties change from point to point (fiber or matrix); at a larger scale the material is assumed homogeneous with "effective properties".
  • Anisotropy: properties depend on direction; much higher along the fibers than transversely.
  • Levels of analysis: micromechanics (fibers and matrix) → lamina macromechanics → laminate → structure.
  • Coupling: in composites, normal stress may produce shear strain and in-plane force may bend the plate; a phenomenon that does not exist in metals.
Key pointComposites' impressive numbers are valid only along the fibers. The transverse and shear strengths of a unidirectional ply are usually tens of times lower than the longitudinal strength; successful composite design means managing this anisotropy.
NABAK CompositePage 3 of 20
Mechanics of FRP Composite Materials
Principles of Composite Material Mechanics

2Constituents: fibers, matrix and interface

Reinforcing fibers

FibersDensityTensile modulus (GPa)Strength (GPa)Feature
E-glass2.54–2.6~72About 3.4 (pristine)Cheap, isotropic, insulating; the most common FRP fiber
S-glass~2.49~86~4.5Higher strength
Carbon (standard)~1.8~230~3.5–5Anisotropic; transverse modulus much lower than longitudinal
Aramid (Kevlar)~1.44~70–125~3.6Tough; weak in compression
Basalt~2.7~85–90~3–4.8Glass substitute with better thermal resistance

Matrices

  • Thermosets: polyester, vinyl ester, epoxy, phenolic, bismaleimide and polyimide. A crosslinked network, chemical and thermal resistance, but relative brittleness. Modulus about 3 to 4 GPa.
  • Thermoplastics: polypropylene, nylon, PPS, PEEK. Toughness, reprocessability and recyclability.
  • Metal and ceramic: for high temperatures; outside the main focus of FRP composites.

Fiber–matrix interface

Load transfer from matrix to fibers takes place through the interface. Adhesion is controlled with sizing and a silane coupling agent (for glass) or surface treatment (for carbon). Weak adhesion reduces transverse and shear strength; very strong adhesion may reduce toughness by eliminating energy dissipation paths (fiber pull-out).

Manufacturing methods from a mechanics perspective

The book examines composite manufacturing methods (lay-up, prepreg and autoclave, RTM, filament winding, pultrusion, SMC molding and injection) in terms of the fiber arrangement, volume fraction, voids and residual stress they create; because all of these are inputs to mechanical analysis.

Vf + Vm + Vv = 1     ρc = ρf·Vf + ρm·Vm
Key pointFiber volume fraction (Vf) and void content (Vv) are the two key numbers of any composite. No mechanical calculation is reliable without knowing the actual Vf (by burn-off or acid digestion testing).
NABAK CompositePage 4 of 20
Mechanics of FRP Composite Materials
Principles of Composite Material Mechanics

3Anisotropy and material symmetry

In general, the generalized Hooke's law relates stress and strain with a 6×6 stiffness matrix. Because of symmetry (existence of strain energy), this matrix has at most 21 independent constants. Each plane of material symmetry reduces the number of constants:

σ_i = C_ij·ε_j     ε_i = S_ij·σ_j     [S] = [C]⁻¹    (i, j = 1…6)
Material typeSymmetryNumber of independent constantsExample
Fully anisotropic (triclinic)No plane of symmetry21—
MonoclinicOne plane of symmetry13Off-axis ply in the reference system
OrthotropicThree mutually perpendicular planes of symmetry9Fabric ply, wood
Transversely isotropicPlane 2-3 isotropic5Unidirectional fiber ply
IsotropicAll directions identical2Metals, neat resin, glass

Engineering constants of a unidirectional ply

For a transversely isotropic ply, the five independent constants are usually chosen as: E₁ (longitudinal modulus), E₂ (transverse modulus), ν₁₂ (major Poisson's ratio), G₁₂ (in-plane shear modulus) and ν₂₃ (or G₂₃). Plane stress analysis needs only the four constants E₁, E₂, ν₁₂ and G₁₂.

ν₂₁ / E₂ = ν₁₂ / E₁ (reciprocity / symmetry of the compliance matrix)

Conceptual notes

  • In an orthotropic material in its principal axes, normal stress produces only normal strain (no shear coupling).
  • If the loading axes do not coincide with the material's principal axes, the material shows "apparently anisotropic" behavior with shear-normal coupling.
  • Poisson's ratios in composites do not have the metals' restriction (less than 0.5), but they must satisfy the positive energy conditions.
Key pointKnowing the symmetry type determines the number of tests needed to characterize a composite. For in-plane design of a unidirectional ply, four engineering constants are enough.
NABAK CompositePage 5 of 20
Mechanics of FRP Composite Materials
Principles of Composite Material Mechanics

4Stress-strain relations of the orthotropic lamina

A thin composite ply (lamina) is usually analyzed in plane stress: σ₃, τ₁₃ and τ₂₃ are assumed zero. This assumption is the basis of classical lamination theory.

Compliance matrix in principal axes

ε₁ = σ₁/E₁ − ν₂₁·σ₂/E₂     ε₂ = −ν₁₂·σ₁/E₁ + σ₂/E₂     γ₁₂ = τ₁₂/G₁₂

Reduced stiffness matrix [Q]

Q₁₁ = E₁/(1−ν₁₂ν₂₁)   Q₂₂ = E₂/(1−ν₁₂ν₂₁)   Q₁₂ = ν₁₂E₂/(1−ν₁₂ν₂₁)   Q₆₆ = G₁₂
{σ₁, σ₂, τ₁₂}ᵀ = [Q]·{ε₁, ε₂, γ₁₂}ᵀ

Numerical example: a glass/epoxy ply

With E₁=40 GPa, E₂=10 GPa, ν₁₂=0.28 and G₁₂=4 GPa: ν₂₁ = 0.28×10/40 = 0.07; 1−ν₁₂ν₂₁ ≈ 0.980. As a result Q₁₁≈40.8, Q₂₂≈10.2, Q₁₂≈2.86 and Q₆₆=4 GPa. The Q₁₁/Q₂₂ ratio is about 4 for glass and about 15 to 20 for carbon/epoxy, showing much stronger anisotropy.

Why a "reduced" stiffness matrix?

Because it is obtained from the 3D matrix [C] by eliminating the thickness components (plane stress assumption). Note that Q_ij is not equal to C_ij.

Key pointThe [Q] matrix is the "mechanical signature" of each composite ply; it is built from four engineering constants, and all later laminate calculations (the ABD matrix) start from it.
NABAK CompositePage 6 of 20
Mechanics of FRP Composite Materials
Principles of Composite Material Mechanics

5Axis transformation and off-axis behavior

In a laminate, plies are laid at different angles (θ) to the reference axis x. To add up their contributions, stresses, strains and the stiffness matrix must be transformed to the reference system.

{σx, σy, τxy}ᵀ = [T]⁻¹{σ₁, σ₂, τ₁₂}ᵀ     [Q̄] = [T]⁻¹[Q][T]⁻ᵀ (with engineering shear strain)

The transformed stiffness matrix [Q̄] generally has six non-zero components; the Q̄₁₆ and Q̄₂₆ components are the "shear coupling": tension in the x direction produces shear strain.

Off-axis modulus

1/Ex = cos⁴θ/E₁ + (1/G₁₂ − 2ν₁₂/E₁)·sin²θ·cos²θ + sin⁴θ/E₂

This relation shows that stiffness drops sharply with a small rotation away from the fiber direction. For carbon/epoxy, the modulus at 15 to 20 degrees may fall to less than half the 0-degree value. For some materials, Ex at an intermediate angle even falls below E₂.

Shear coupling coefficient

The ratio η_xy,x = γxy/εx (under uniaxial stress σx) quantifies the coupling. In a tensile test of an off-axis specimen, this coupling causes S-shaped distortion of the specimen between the grips; that is why the specimen's length-to-width ratio and grip type matter.

Invariants

The components of Q̄ can be expressed with invariants U₁ to U₅ that do not depend on angle. This form simplifies parametric analysis and quasi-isotropic laminate design: the stiffness of a quasi-isotropic laminate depends only on U₁, U₄ and U₅.

Ply angleBehavior
0°Highest tensile stiffness and strength in the x direction
±45°Highest in-plane shear stiffness; for torsional and shear loads
90°Transverse stiffness; controls Poisson's ratio and early matrix cracking
Key pointA small deviation of fibers from the design direction (waviness or inaccurate placement in manufacturing) causes a noticeable loss of stiffness and strength. Controlling fiber direction in production is a mechanical requirement, not a cosmetic one.
NABAK CompositePage 7 of 20
Mechanics of FRP Composite Materials
Principles of Composite Material Mechanics

6Micromechanics of stiffness: rule of mixtures and Halpin-Tsai

Micromechanics predicts the effective properties of a ply from the properties of the fiber, the matrix and the volume fraction. The book starts from simple (mechanics of materials) models and goes on to elasticity and finite element models.

Mechanics of materials model (representative volume element)

E₁ = Ef·Vf + Em·Vm     (iso-strain / Voigt)
1/E₂ = Vf/Ef + Vm/Em     1/G₁₂ = Vf/Gf + Vm/Gm     (iso-stress / Reuss)
ν₁₂ = νf·Vf + νm·Vm

The rule of mixtures is very accurate for E₁ and ν₁₂. But the inverse model underestimates E₂ and G₁₂, because the assumption of equal stress in fiber and matrix is not realistic.

Halpin-Tsai semi-empirical equations

M/Mm = (1 + ξ·η·Vf) / (1 − η·Vf)     η = (Mf/Mm − 1) / (Mf/Mm + ξ)

M can be E₂, G₁₂ or ν₂₃. The reinforcement parameter ξ depends on fiber geometry and arrangement (e.g. about 2 for E₂ and 1 for G₁₂ for circular fibers in a square array). ξ=0 reduces to the inverse rule and ξ→∞ to the direct rule of mixtures.

Numerical example

E-glass (Ef=72 GPa) in epoxy (Em=3.5 GPa) with Vf=0.6: E₁ = 43.2+1.4 ≈ 44.6 GPa. With the inverse rule E₂ ≈ 8.2 GPa, and with Halpin-Tsai (ξ=2): Ef/Em≈20.6, η≈0.867, E₂ ≈ 3.5×(1+1.04)/(1−0.52) ≈ 14.9 GPa, which is closer to experimental data.

Other methods

  • Elasticity models: concentric cylinders, variational bounds (Hashin-Shtrikman).
  • Unit cell finite elements: square or hexagonal arrays; allow study of stress concentrations in the matrix and interface.
  • Random fiber arrangements and the effect of voids on properties.
Key pointLongitudinal properties are fiber-controlled and transverse and shear properties are matrix-controlled. To improve longitudinal stiffness you need better fibers or higher Vf; to improve transverse and shear behavior you need a better resin and a stronger interface.
NABAK CompositePage 8 of 20
Mechanics of FRP Composite Materials
Principles of Composite Material Mechanics

7Lamina strength and failure criteria

A unidirectional composite ply has five basic strengths that must be determined separately by testing; unlike metals, tensile and compressive strengths are not equal:

SymbolDefinitionTypical glass/epoxy value (MPa)
s_L(+)Longitudinal tensile~1000
s_L(−)Longitudinal compressive~600
s_T(+)Transverse tensile~30–40
s_T(−)Transverse compressive~120–140
s_LTIn-plane shear~40–70

Failure criteria under multiaxial stress

  • Maximum stress: failure when any stress component in principal axes reaches the corresponding strength. Simple and identifies the failure mode, but ignores stress interaction.
  • Maximum strain: similar, in terms of limiting strains; partly accounts for the Poisson effect.
  • Tsai-Hill: a distortion energy criterion modified for orthotropic materials; interactive:
(σ₁/s_L)² − σ₁σ₂/s_L² + (σ₂/s_T)² + (τ₁₂/s_LT)² = 1
  • Tsai-Wu (tensor polynomial): accounts for the tension-compression difference with linear terms:
F₁σ₁ + F₂σ₂ + F₁₁σ₁² + F₂₂σ₂² + F₆₆τ₁₂² + 2F₁₂σ₁σ₂ = 1
F₁ = 1/s_L(+) − 1/s_L(−)   F₁₁ = 1/(s_L(+)·s_L(−))   F₆₆ = 1/s_LT²

The interaction coefficient F₁₂ requires a biaxial test, and the approximation F₁₂ ≈ −½√(F₁₁F₂₂) is usually used.

Off-axis failure

By transforming the uniaxial stress σx to principal axes, the strength of a θ-degree ply is predicted. At small angles fiber failure dominates; at intermediate angles shear failure; at large angles transverse matrix failure. Interactive criteria give a smoother curve, closer to experiment.

NoteThe book also mentions mechanism-based failure criteria such as Hashin and Puck, which separate fiber and matrix failure; the World-Wide Failure Exercise showed that no criterion is best in all cases.
Key pointNegative and positive shear stress in principal axes have the same effect, but transverse tensile stress is much more dangerous than compressive. Always apply the failure criterion in the material's principal axes, not in the structural axes.
NABAK CompositePage 9 of 20
Mechanics of FRP Composite Materials
Principles of Composite Material Mechanics

8Micromechanics of strength

Longitudinal tensile strength

If the fiber failure strain is lower than the matrix's (the common case in FRP), failure starts with fiber rupture:

s_L(+) = s_f·Vf + σ'_m·(1 − Vf)     (σ'_m = matrix stress at fiber failure strain)

At very low volume fractions, the matrix still carries the load after the fibers break; so there is a minimum volume fraction (V_min) below which the fibers do not increase strength, and a critical volume fraction (V_crit) above which the composite is stronger than the matrix. In FRP with a weak resin, these values are small.

Statistical nature of fiber strength

Fiber strength follows a Weibull distribution and decreases with length (a higher probability of flaws). In a composite, broken fibers pick up load again through matrix shear; ultimate failure results from the accumulation of random breaks and their clustering.

Longitudinal compressive strength

In compression, fibers behave like slender beams on an elastic matrix foundation and may undergo microbuckling. The Rosen model predicts two modes: the "extension" mode (out-of-phase fibers, low Vf) and the "shear" mode (in-phase fibers, typical Vf):

s_L(−) ≈ Gm / (1 − Vf)     (Rosen, shear mode)

This model overestimates; initial fiber misalignment and nonlinear shear behavior of the matrix sharply lower the actual compressive strength and lead to "kink bands". That is why the compressive strength of composites is usually lower than the tensile.

Transverse and shear strength

These are controlled by the matrix and interface. Stiff fibers create strain concentration in the matrix between fibers; so the transverse strength of a composite can even be lower than that of the neat resin. The strain magnification factor increases with Vf. Voids and weak adhesion also reduce transverse strength.

Key pointStraight, aligned fibers are vital for compressive strength. Fiber waviness in manufacturing (e.g. in pultrusion or lay-up) is one of the main reasons compressive strength is low relative to the theoretical value.
NABAK CompositePage 10 of 20
Mechanics of FRP Composite Materials
Principles of Composite Material Mechanics

9Thermal and moisture (hygrothermal) behavior

In real environments, FRP composites face temperature changes and moisture absorption. These two factors both create "free" (stress-free) strains and change the mechanical properties of the matrix.

Hygrothermal strains

{ε} = [S]{σ} + {α}·ΔT + {β}·Δc

α are the coefficients of thermal expansion and β the coefficients of moisture expansion in directions 1 and 2. In an off-axis ply, a thermal shear strain also appears.

Micromechanics of expansion coefficients

α₁ = (Ef·αf·Vf + Em·αm·Vm) / (Ef·Vf + Em·Vm)     (Schapery)

Stiff fibers restrain longitudinal expansion; so α₁ is close to the fiber's and small (and in carbon/epoxy it may even be negative and near zero), but α₂ is large and close to the matrix's. This difference is the source of residual stress between plies after cooling from the cure temperature.

Moisture diffusion: Fick's law

∂c/∂t = D_z·∂²c/∂z²     M(t) ≈ M_m·[1 − exp(−7.3·(D_z·t/h²)^0.75)]
  • The diffusion coefficient D increases with temperature in Arrhenius fashion; accelerated tests at high temperature are based on this.
  • Initial absorption is proportional to the square root of time and then reaches the equilibrium moisture content M_m, which depends on the ambient relative humidity.
  • The time to reach saturation increases with the square of thickness; thick parts take years to saturate.

Effect on properties

Moisture softens the matrix and lowers the glass transition temperature (Tg). The hot/wet combination is the worst condition for matrix-controlled properties (longitudinal compression, transverse and shear). Fiber-controlled properties (longitudinal tension) are less sensitive, although glass fibers may suffer stress corrosion in the presence of moisture and stress.

Key pointComposite design must use "hot-wet" properties, not dry laboratory properties. Choosing a resin with high Tg and low water absorption (such as a suitable vinyl ester or epoxy) and a surface veil increases the environmental safety margin.
NABAK CompositePage 11 of 20
Mechanics of FRP Composite Materials
Principles of Composite Material Mechanics

10Discontinuous fiber composites and nanocomposites

In short or chopped fiber composites (such as SMC, BMC, injection-molded parts and random mats in FRP profiles), load must be transferred from the matrix to the fibers through shear at the interface. This transfer is incomplete at both ends of each fiber.

Shear lag analysis

The Cox model shows that the tensile stress in a fiber rises from zero at both ends and approaches its maximum in the middle, while the interfacial shear stress peaks at the ends. The length of fiber over which stress is not fully built up is called the "ineffective length".

Critical fiber length (Kelly-Tyson)

l_c = s_f·d / (2·τ_y)

τ_y is the interfacial shear strength or the matrix shear yield stress. If the fiber is shorter than l_c, it never reaches its strength and is pulled out of the matrix; if it is much longer, behavior approaches that of continuous fibers. This is why the length-to-diameter ratio (l/d) is decisive in short-fiber composites.

Stiffness and strength of aligned discontinuous fibers

The Halpin-Tsai equations with ξ = 2(l/d) are used for E₁; as l/d increases, the longitudinal modulus approaches the rule of mixtures. Strength is calculated with the "average fiber stress" along its length, which is lower than the full strength.

Randomly oriented fibers

For in-plane random fibers, averaging over all angles or the following approximate relation is used:

E_random ≈ (3/8)·E₁ + (5/8)·E₂

The material is nearly isotropic in the plane, but its stiffness is much lower than a unidirectional ply.

Nanocomposites

Carbon nanotubes, graphene and nanoclay particles with very high aspect ratios can improve matrix properties at small loadings. Challenges: uniform dispersion, agglomeration, interfacial adhesion and misalignment; so the actual improvement is usually less than ideal micromechanics predicts. Their important application is reinforcing the matrix in multiscale (hierarchical) composites and adding multifunctional properties such as conductivity.

Key pointIn short-fiber composites, interface quality and fiber length are as important as volume fraction; fiber breakage during compounding or injection sharply reduces properties.
NABAK CompositePage 12 of 20
Mechanics of FRP Composite Materials
Principles of Composite Material Mechanics

11Classical lamination theory and the ABD matrix

Classical lamination theory (Classical Lamination Theory, CLT) is the heart of composite mechanics and predicts the behavior of a multi-ply laminate from the properties and angle of each ply.

Assumptions

  • The laminate is thin and the plies are perfectly bonded (no slip between plies).
  • Kirchhoff assumption: a line normal to the mid-plane stays straight and normal (transverse shear strains zero).
  • Each ply is in plane stress and linear elastic.

Strain field

{ε} = {ε⁰} + z·{κ}

The strain at any point equals the mid-plane strain plus the distance from the mid-plane times the curvature. Strain is linear through the thickness, but stress is piecewise and discontinuous because of the different [Q̄] of the plies.

Force and moment relations: the ABD matrix

{N} = [A]{ε⁰} + [B]{κ}     {M} = [B]{ε⁰} + [D]{κ}
A_ij = Σ Q̄_ij(z_k − z_k−1)   B_ij = ½Σ Q̄_ij(z_k² − z_k−1²)   D_ij = ⅓Σ Q̄_ij(z_k³ − z_k−1³)
MatrixMeaningDesign note
[A] extensional stiffnessIn-plane force → in-plane strainDoes not depend on ply sequence
[B] couplingIn-plane force → bending and twistingZero in a symmetric laminate
[D] bending stiffnessMoment → curvatureOuter plies contribute more (z³)
A₁₆, A₂₆Extension-shear couplingZero in a balanced laminate
D₁₆, D₂₆Bend-twist couplingSmall but usually non-zero in ±θ laminates

Solution procedure

By inverting the ABD matrix, the mid-plane strains and curvatures are calculated from the loads; then the strain in each ply in x-y axes, transformation to 1-2 axes and the stress in each ply are obtained so the failure criterion can be applied.

Key pointA non-zero [B] matrix means the laminate warps during cure and cooling or under simple tension. A laminate symmetric about the mid-plane eliminates this unwanted coupling, and this is the golden rule of design.
NABAK CompositePage 13 of 20
Mechanics of FRP Composite Materials
Principles of Composite Material Mechanics

12Layup design and laminate strength

Layup code and laminate types

The code [0/±45/90]s means plies at 0, +45, −45 and 90 degrees in that order, then mirrored about the mid-plane (s = symmetric).

Laminate typeDefinitionMechanical characteristic
SymmetricGeometric and material mirror image about the mid-plane[B]=0; no thermal warping
BalancedFor every +θ, a −θ of the same thicknessA₁₆=A₂₆=0; no extension-shear coupling
Cross-plyOnly 0 and 90 degreesNo shear coupling; low shear stiffness
Angle-ply±θHigh shear stiffness at ±45
Quasi-isotropicE.g. [0/±45/90]s or [0/±60]s[A] like an isotropic material in-plane; [D] not necessarily isotropic

Residual thermal stresses

After curing at high temperature and cooling, plies at different angles want to contract differently (α₁ small, α₂ large); because they are bonded together, residual stress arises. In CLT this effect enters through "equivalent thermal forces and moments" (N^T, M^T). Residual transverse tensile stress in 90-degree plies can approach matrix cracking even without external load.

Laminate strength: progressive failure

  1. First-ply failure (FPF): as load increases, the stress in each ply is checked and the first ply to meet the failure criterion (e.g. Tsai-Wu) is identified; usually matrix cracking in the 90-degree plies.
  2. Stiffness reduction: the properties of the failed ply (e.g. E₂ and G₁₂) are reduced or set to zero.
  3. Re-analysis with the new ABD matrix and continued load increase.
  4. Last-ply failure (LPF): when the main load-bearing plies (usually 0 degrees) break, the laminate collapses.

This is why the laminate load-strain plot has a "knee": after FPF the slope decreases but the laminate still carries load.

Empirical design rules

  • Symmetric and balanced layup, unless coupling is deliberately wanted.
  • At least about 10% of plies in each of the 0, ±45 and 90 directions to carry unforeseen loads.
  • Avoid stacking many same-orientation plies together (increases interlaminar stress and cracking).
  • ±45 plies on the outer surface for resistance to impact and buckling.
Key pointFirst-ply failure is usually not "structural failure", but it is the start of damage, moisture ingress and reduced fatigue life. In corrosion-resistant applications (such as FRP tanks and profiles in chemical environments), design is often based on FPF or a strain limit.
NABAK CompositePage 14 of 20
Mechanics of FRP Composite Materials
Principles of Composite Material Mechanics

13Composite beams and plates: bending, buckling and vibration

The book extends CLT to structural analysis. The plate equilibrium equations are combined with the A, B and D matrices. For a symmetric, specially orthotropic plate (D₁₆=D₂₆=0):

D₁₁·∂⁴w/∂x⁴ + 2(D₁₂ + 2D₆₆)·∂⁴w/∂x²∂y² + D₂₂·∂⁴w/∂y⁴ = q(x,y)

Flexure

For a simply supported rectangular plate, the Navier solution with a double Fourier series gives the deflection. Deflection is proportional to the inverse of D, and D grows with the cube of thickness; so increasing thickness or placing stiff plies at the outer surface is the most effective way to reduce deflection. In laminated beams, the "effective bending stiffness" is obtained from the inverse of D (i.e. 1/D*₁₁), not from a simple E·I.

Buckling

N_x,cr = (π²/b²)·[ D₁₁(m b/a)² + 2(D₁₂+2D₆₆) + D₂₂(a/(m b))² ]

The critical buckling load of a plate in compression depends on bending stiffness and aspect ratio. Local buckling of flanges and webs in thin-walled composite profiles (such as FRP I-sections and channels) is often the governing design mode, because the modulus is lower than steel's.

Free vibration

Natural frequencies are proportional to √(D/ρh). Composites' high stiffness-to-density ratio raises natural frequency; an advantage for rotating and aircraft structures.

Effect of transverse shear

In composites, the transverse shear moduli (G₁₃, G₂₃) are very low compared with E₁. In thick laminates or short beams, shear deformation contributes significantly to deflection and the Kirchhoff assumption introduces error; first-order (Mindlin-Reissner) or higher-order theories are needed.

Note for FRP profile designIn pultruded beams with E of about 20 to 30 GPa and a shear modulus of about 3 to 4 GPa, the shear contribution to deflection in short beams can exceed ten percent; calculating deflection with Timoshenko beam theory is recommended.
Key pointIn composite structures, stiffness (deflection and buckling) governs more often than strength. Section design, thickness and the placement of stiff plies are the designer's most important tools.
NABAK CompositePage 15 of 20
Mechanics of FRP Composite Materials
Principles of Composite Material Mechanics

14Viscoelasticity, creep and damping

The polymer matrix behaves in a time- and temperature-dependent way; so FRP composites, especially in matrix-controlled properties, show creep and stress relaxation and dissipate energy in vibration.

Creep and stress relaxation

  • Creep: increase in strain with time under constant stress; described by the creep compliance function S(t).
  • Stress relaxation: decrease in stress with time under constant strain; with the relaxation modulus E(t).
  • Spring and dashpot models: Maxwell (series), Kelvin-Voigt (parallel), the standard linear solid and Prony series for real data.

Boltzmann superposition principle

ε(t) = ∫ S(t − τ)·(dσ/dτ) dτ

In linear viscoelasticity, the response to a load history equals the sum of the responses to each load increment. The elastic-viscoelastic correspondence principle allows elastic solutions (including micromechanics and CLT) to be converted to viscoelastic problems in Laplace space.

Time-temperature superposition

In "thermorheologically simple" materials, raising the temperature is equivalent to speeding up time. With a shift factor a_T (Arrhenius below Tg or WLF near and above Tg), short-term curves at different temperatures are combined into a "master curve" at a reference temperature, and behavior over decades is predicted from tests lasting a few days. Moisture and stress have a similar shifting effect.

Dynamic behavior and damping

E* = E' + i·E''     η = E''/E' = tan δ

E' is the storage modulus and E'' the loss modulus. DMA testing is used to determine Tg (tan δ peak) and damping. Composite damping is several times that of metals and higher in the transverse and shear directions than longitudinally. The book shows that structural damping can be designed by choosing ply angles and adding viscoelastic layers.

Key pointFor permanent loads (such as the weight of equipment on FRP grating or beams), long-term properties that account for creep must be used; the effective long-term modulus can be noticeably lower than the short-term modulus, especially at high temperature and humidity.
NABAK CompositePage 16 of 20
Mechanics of FRP Composite Materials
Principles of Composite Material Mechanics

15Fracture mechanics and delamination

Strength-based failure criteria assume the material is flawless; but real composites have cracks, voids and impact damage. Linear elastic fracture mechanics (LEFM) analyzes the growth of these flaws.

Basic concepts

K_I = Y·σ·√(πa)     G = (P²/2b)·dC/da     crack grows when G ≥ G_c
  • Stress intensity factor (K): the crack-tip stress field; in anisotropic materials it depends on the elastic constants.
  • Strain energy release rate (G): energy released per unit area of crack growth; more practical than K for composites.
  • Fracture modes: mode I (opening), II (sliding shear), III (tearing) and mixed modes.

Interlaminar stresses and the free edge

CLT assumes zero stress between plies, but near free edges, holes and ply drops, interlaminar stresses (σz, τxz, τyz) appear because of mismatches in the plies' Poisson's ratios and shear coupling, and they can initiate delamination. The stacking sequence has a large effect on the sign and magnitude of σz at the edge.

Interlaminar toughness tests

TestModeStandard
Double cantilever beam (DCB)Mode I, G_IcASTM D5528
End-notched flexure (ENF)Mode II, G_IIcASTM D7905
Mixed-mode bending (MMB)Combined I/IIASTM D6671

Toughness and energy dissipation mechanisms

Fiber pull-out, fiber bridging across the crack, interface debonding and multiple matrix cracking absorb energy and increase toughness. Tough matrices (thermoplastic or rubber-modified epoxy), through-thickness stitching and 3D fibers raise resistance to delamination. G_IIc is usually several times G_Ic.

Key pointDelamination is the Achilles' heel of laminates, especially after impact or at edges and holes. Compression after impact (CAI) strength is an important design criterion for structural composites.
NABAK CompositePage 17 of 20
Mechanics of FRP Composite Materials
Principles of Composite Material Mechanics

16Mechanical testing of composites

Every composite mechanics model depends on test data. The book describes constituent and lamina tests, emphasizing the particular challenges of anisotropic materials.

PropertyTest / standardKey point
Lamina tension (E₁, E₂, ν₁₂, strength)ASTM D3039Rectangular specimen with tabs; precise alignment
CompressionASTM D3410, D6641Preventing global buckling of the specimen; shear or combined loading
In-plane shear (G₁₂)ASTM D3518 (±45), D5379 (V-notch), D7078±45 is simple; V-notch gives purer shear
Apparent interlaminar shearASTM D2344 (Short beam)Quality control test; not precise design data
FlexureASTM D790, D7264Combination of tension, compression and shear
Fiber volume fraction and voidsASTM D3171, D2734Input to all models
Single fiber tensionASTM D3379 / C1557Weibull distribution; gauge length effect
Interfacial adhesionFiber pull-out, fragmentation, microdropletEstimating τ and critical length
Tg and dampingDMAtan δ peak

Important points in composite testing

  • Back-to-back strain gauges: comparing the strain on both faces of the specimen reveals unwanted bending from misalignment.
  • Valid failure mode: failure in the grip or tab is an invalid result; standards define failure mode codes.
  • Environmental conditions: testing dry and after moisture conditioning at high temperature to determine hot-wet properties.
  • Number of specimens and statistics: composites have more scatter than metals; design allowables (B-basis, A-basis) are set statistically.
  • Non-destructive tests: ultrasonics, thermography and radiography to detect voids and delamination.
Key pointComposite test data depend on direction, manufacturing method, volume fraction and environmental conditions. Always report and check Vf, layup and test conditions alongside every number.
NABAK CompositePage 18 of 20
Mechanics of FRP Composite Materials
Principles of Composite Material Mechanics

17Conclusions, application to FRP profiles and frequently asked questions

Ten golden rules of composite mechanics

  1. Composites are heterogeneous and anisotropic; effective properties and the material's principal axes are the basis of every analysis.
  2. A unidirectional ply in plane stress is described by four constants E₁, E₂, ν₁₂ and G₁₂.
  3. Longitudinal properties are fiber-controlled and transverse and shear properties matrix-controlled.
  4. The rule of mixtures is accurate for E₁; for E₂ and G₁₂ use Halpin-Tsai.
  5. Stiffness and strength drop rapidly with rotation away from the fiber direction.
  6. Compressive strength is limited by microbuckling and fiber misalignment.
  7. CLT and the ABD matrix build laminate behavior from the plies; symmetry and balance eliminate couplings.
  8. Design must use hot-wet and long-term (creep) properties.
  9. Delamination and interlaminar stresses are critical at edges and holes.
  10. Without valid testing and knowing Vf, no mechanical model is reliable.

Application to FRP profile design and production

A pultruded profile combines unidirectional roving with mat or fabric and can be treated as a symmetric laminate. Micromechanics gives each ply's properties; CLT the flange and web stiffness; the failure criterion the strength; and local buckling and shear deflection analysis the capacity of an FRP beam or column. This chain links the product's technical property table to reliable structural design.

Frequently asked questions

What is classical lamination theory? A method for calculating the behavior of a composite laminate from ply properties and angles, relating forces and moments to mid-plane strains and curvatures through the ABD matrix.

What is the rule of mixtures used for? Estimating a ply's longitudinal modulus and Poisson's ratio from fiber and matrix properties and volume fraction; for transverse properties, Halpin-Tsai is more accurate.

What is the Tsai-Wu failure criterion? An interactive quadratic criterion that accounts for the combined effect of ply stresses and the difference between tensile and compressive strength.

Why should a laminate be symmetric? To eliminate extension-bending coupling and prevent warping after cure.

NABAK CompositePage 19 of 20
Mechanics of FRP Composite Materials
Principles of Composite Material Mechanics

18Glossary of composite mechanics terms

English termMeaningShort explanation
Lamina / LaminateLamina / laminateSingle composite ply / ply stack
OrthotropicOrthotropicThree mutually perpendicular planes of symmetry
Transversely isotropicTransversely isotropicUnidirectional ply; 5 independent constants
Reduced stiffness [Q]Reduced stiffnessPlane stress stiffness matrix
Off-axisOff-axisLoading at an angle to the fibers
Shear couplingShear couplingShear strain produced by normal stress
MicromechanicsMicromechanicsPredicting properties from fiber and matrix
Rule of mixturesRule of mixturesVolume-fraction-weighted average
Halpin–TsaiHalpin-TsaiSemi-empirical equations for transverse properties
Tsai–Wu / Tsai–HillTsai-Wu / Tsai-HillInteractive failure criteria
Microbuckling / Kink bandMicrobuckling / kink bandFiber compressive failure
HygrothermalHygrothermalCombined effect of temperature and moisture
Shear lagShear lagLoad transfer in discontinuous fibers
Critical fiber lengthCritical fiber lengthMinimum length for a fiber to reach its strength
CLT / ABD matrixClassical lamination theory / ABD matrixLaminate analysis
Symmetric / BalancedSymmetric / balancedEliminating bending / shear coupling
Quasi-isotropicQuasi-isotropicIsotropic in-plane stiffness
First/Last ply failureFirst / last ply failureProgressive failure analysis
Creep / RelaxationCreep / stress relaxationTime-dependent behavior
Loss factorLoss factorDamping indicator
DelaminationDelaminationCrack between plies
Strain energy release rateStrain energy release rateCrack growth criterion G

Related keywords: composite mechanics, mechanics of composite materials, FRP composites, classical lamination theory, ABD matrix, micromechanics, rule of mixtures, Tsai-Wu criterion, composite strength, laminate, composite testing, FRP profiles, NABAK Composite.

NABAK CompositePage 20 of 20