Practical Analysis of FRP Composite Laminates
Practical Analysis of Composite Laminates

Practical Analysis of Composite Laminates

Practical Analysis of Composite Laminates: A Comprehensive Book Summary

An engineering guide to analyzing FRP composite laminates and plates: classical laminated plate theory, first-order shear deformation theory, the ABD matrix, bending, buckling and vibration of composite plates and beams, the finite element method, failure analysis and layup design principles

Authors of the original book: J. N. Reddy, Antonio Miravete
Publisher: CRC Press — field: structural analysis and design of laminated composites
Prepared for: NABAK Composite

Where does this book stand?

The book is the product of a collaboration between one of the most prominent researchers in composite plate theory (Reddy) and a specialist in industrial composite design (Miravete). Its aim is to bridge rigorous theory and the design engineer's everyday needs: how to define a composite laminate, calculate its stiffness, predict a plate's deflection, buckling load and natural frequency, analyze it with finite elements and finally assess its strength and safety. For FRP product designers, this book is the "analysis toolbox" for laminated structures.

How to use this summary

  • Orange "Key point" boxes state the most important practical conclusion of each chapter for composite analysis.
  • Gold "Note" boxes show how the material applies to designing FRP profiles, panels and composite structures.
  • Notation: direction 1 is along the fibers, x-y are the plate axes, z the thickness, w the deflection, a and b the plate dimensions and h the laminate thickness.
  • The example figures are for understanding trends and are not a substitute for your material data.
NABAK CompositePage 1 of 19
Practical Analysis of FRP Composite Laminates
Practical Analysis of Composite Laminates

Table of Contents

  1. 1Introduction: composite laminates and basic terms
  2. 2Lamina mechanics: stress-strain relations
  3. 3Transformation of stress, strain and stiffness
  4. 4Classical laminated plate theory and the ABD matrix
  5. 5Laminate types, couplings and effective constants
  6. 6Thermal and moisture effects in laminates
  7. 7First-order shear deformation theory (FSDT)
  8. 8Governing equations and boundary conditions of plates
  9. 9Bending of composite plates: Navier and Lévy solutions
  10. 10Buckling of composite plates
  11. 11Free vibration of composite plates
  12. 12Laminated composite beams
  13. 13Finite element analysis of laminates
  14. 14Failure and progressive damage analysis
  15. 15Practical design of laminates and composite structures
  16. 16Conclusions and frequently asked questions
  17. 17Glossary of laminate analysis terms
The book's main message in one sentenceThe behavior of a composite laminate is determined by the sequence and angles of its plies; with a suitable theory (classical for thin, shear for thick) and the right numerical tools, the deflection, buckling, vibration and failure of any FRP plate or beam can be predicted before it is built.
NABAK CompositePage 2 of 19
Practical Analysis of FRP Composite Laminates
Practical Analysis of Composite Laminates

1Introduction: composite laminates and basic terms

Fiber-reinforced polymer (FRP) composites are usually made in layers. Each layer (lamina or ply) consists of unidirectional fibers or fabric in a polymer matrix, and stacking several plies at different angles forms a composite laminate. The art of composite design lies in choosing the number, material, thickness and sequence of these plies.

Key terms

TermDefinition
Lamina (single ply)A thin layer with aligned or woven fibers; the basic unit of analysis
LaminateA set of bonded plies with different orientations
Layup codeE.g. [0/45/−45/90]s: angles from the top, and s means symmetric
Mid-planeThe reference plane at mid-thickness (z = 0)
Material axes 1-2-31 along the fibers, 2 perpendicular to them in the plane, 3 through the thickness
Structural axes x-y-zReference axes of the plate or beam
HybridA laminate with more than one fiber type (e.g. glass and carbon)
SandwichTwo composite skins with a light core (foam, honeycomb, balsa wood)

Advantages and challenges of composite laminates

  • Advantages: high specific strength and stiffness, corrosion resistance, good fatigue, directional tailoring of properties, fewer parts.
  • Challenges: anisotropy, unusual couplings (extension-bending, bend-twist), sensitivity to interlaminar stresses and delamination, and analytical complexity.

Applications

The book reviews applications in aerospace, automotive, marine, building and infrastructure, sporting goods and the chemical industries. In all these fields, the main structural elements — composite plates, shells and beams — are examined with the same laminate analysis tools.

Key pointIn composite analysis, "material" and "structure" cannot be separated: changing the ply sequence without changing material or weight noticeably changes the laminate's bending stiffness and buckling behavior.
NABAK CompositePage 3 of 19
Practical Analysis of FRP Composite Laminates
Practical Analysis of Composite Laminates

2Lamina mechanics: stress-strain relations

Laminate analysis starts with the behavior of a single ply. A unidirectional ply is orthotropic (more precisely, transversely isotropic) in its material axes. The 3D Hooke's law for an orthotropic material has 9 independent constants:

E₁, E₂, E₃, G₁₂, G₁₃, G₂₃, ν₁₂, ν₁₃, ν₂₃     νij/Ei = νji/Ej

Plane stress state

In a thin ply, σ₃₃ is negligible. Dropping it, the in-plane relation is expressed with the reduced stiffness matrix; the transverse shear stresses are written separately (they are needed for shear theory):

σ₁ = Q₁₁ε₁ + Q₁₂ε₂    σ₂ = Q₁₂ε₁ + Q₂₂ε₂    τ₁₂ = Q₆₆γ₁₂    τ₂₃ = Q₄₄γ₂₃    τ₁₃ = Q₅₅γ₁₃
Q₁₁ = E₁/(1−ν₁₂ν₂₁)   Q₁₂ = ν₁₂E₂/(1−ν₁₂ν₂₁)   Q₂₂ = E₂/(1−ν₁₂ν₂₁)   Q₆₆ = G₁₂   Q₄₄ = G₂₃   Q₅₅ = G₁₃

Typical properties of common plies

MaterialE₁ (GPa)E₂ (GPa)G₁₂ (GPa)ν₁₂E₁/E₂
Unidirectional glass/epoxy~39–45~8–13~4–5~0.26–0.3~3–5
Unidirectional carbon/epoxy~130–180~9–10~5–7~0.28–0.3~15–20
Aramid/epoxy~76~5.5~2.3~0.34~14

In plate theory studies (and in this book), hypothetical materials with E₁/E₂ = 25 or 40 and G₁₂ = G₁₃ = 0.5E₂, G₂₃ = 0.2E₂ and ν₁₂ = 0.25 are widely used so that the effect of strong anisotropy can be clearly seen.

Micromechanics at a glance

Ply constants are estimated from fiber and matrix properties with the rule of mixtures (E₁ and ν₁₂) and inverse or Halpin-Tsai relations (E₂ and G₁₂), but for design, experimental measurement is preferred.

Key pointThe ratios E₁/E₂ and E₁/G₁₃ are the main indicators of a laminate's sensitivity to shear deformation and couplings; the larger they are, the greater the error of classical theory and the more serious the need for shear theory.
NABAK CompositePage 4 of 19
Practical Analysis of FRP Composite Laminates
Practical Analysis of Composite Laminates

3Transformation of stress, strain and stiffness

Each ply in the laminate lies at an angle θ to the x axis. To add up the plies' contributions, each ply's stiffness matrix must be transformed to the structural axes. With m = cosθ and n = sinθ:

Q̄₁₁ = Q₁₁m⁴ + 2(Q₁₂+2Q₆₆)m²n² + Q₂₂n⁴
Q̄₁₂ = (Q₁₁+Q₂₂−4Q₆₆)m²n² + Q₁₂(m⁴+n⁴)    Q̄₂₂ = Q₁₁n⁴ + 2(Q₁₂+2Q₆₆)m²n² + Q₂₂m⁴
Q̄₁₆ = (Q₁₁−Q₁₂−2Q₆₆)m³n + (Q₁₂−Q₂₂+2Q₆₆)mn³    Q̄₂₆ = (Q₁₁−Q₁₂−2Q₆₆)mn³ + (Q₁₂−Q₂₂+2Q₆₆)m³n
Q̄₆₆ = (Q₁₁+Q₂₂−2Q₁₂−2Q₆₆)m²n² + Q₆₆(m⁴+n⁴)
Q̄₄₄ = Q₄₄m² + Q₅₅n²   Q̄₅₅ = Q₅₅m² + Q₄₄n²   Q̄₄₅ = (Q₅₅−Q₄₄)mn

Engineering interpretation

  • Q̄₁₆ and Q̄₂₆ are shear-normal coupling terms; they are zero for θ = 0° and 90° and have opposite signs for ±θ. This property is the basis of the balanced laminate concept.
  • Q̄₆₆ is maximum at θ = ±45°; ±45 degree plies provide the laminate's shear stiffness.
  • To check failure, stresses must be transformed back to material axes; stresses in x-y axes alone are not enough to judge strength.

Stress and strain transformation

{σ₁, σ₂, τ₁₂} = [T]{σx, σy, τxy}     [T] = [[m², n², 2mn], [n², m², −2mn], [−mn, mn, m²−n²]]

When working with engineering shear strain (γ = 2ε), the factor of 2 must be respected in the strain transformation (Reuter matrix); this is one of the common errors in programming laminate analysis.

Off-axis engineering constants

1/Ex = m⁴/E₁ + (1/G₁₂ − 2ν₁₂/E₁)m²n² + n⁴/E₂

For a carbon/epoxy ply, the modulus at 30 degrees is only about 15 percent of the 0-degree modulus; this strong sensitivity to angle shows the importance of controlling fiber orientation in manufacturing.

Key pointAll laminate calculations are done with [Q̄], but all strength judgments in material axes 1-2. This back-and-forth transformation is the backbone of every composite analysis program.
NABAK CompositePage 5 of 19
Practical Analysis of FRP Composite Laminates
Practical Analysis of Composite Laminates

4Classical laminated plate theory and the ABD matrix

Classical laminated plate theory (CLPT) extends Kirchhoff theory to composite plates and is the simplest laminate analysis theory.

Displacement field

u = u₀(x,y,t) − z·∂w₀/∂x    v = v₀ − z·∂w₀/∂y    w = w₀(x,y,t)

Assumption: lines normal to the mid-plane remain straight, inextensible and normal to the mid-plane after deformation; the transverse shear strains γxz and γyz are therefore zero.

{ε} = {ε⁰} + z{κ}    ε⁰x = ∂u₀/∂x   κx = −∂²w₀/∂x²   κxy = −2∂²w₀/∂x∂y

Stress resultants and the ABD matrix

(Nx, Ny, Nxy) = ∫ σ dz     (Mx, My, Mxy) = ∫ σ·z dz
{N; M} = [[A, B], [B, D]]·{ε⁰; κ}
(Aij, Bij, Dij) = Σₖ ∫ Q̄ij⁽ᵏ⁾·(1, z, z²) dz

Step-by-step calculation procedure

  1. Determine Q for each ply from the engineering constants.
  2. Transform to Q̄ with each ply's angle.
  3. Determine the z coordinates of the ply surfaces from the mid-plane.
  4. Calculate A, B and D and form the 6×6 matrix.
  5. Invert ABD and calculate mid-plane strains and curvatures from the loads.
  6. Calculate strain and stress at the top and bottom of each ply, transform to material axes and apply the failure criterion.

Interpretive notes

  • [A] depends only on ply thickness and angle, not their sequence.
  • [D] depends strongly on ply sequence; outer plies, weighted by z², contribute most.
  • [B] results from asymmetry and is zero in a symmetric laminate.
  • Strain is continuous and linear through the thickness, but stress jumps at ply interfaces.
Key pointTo increase a laminate's bending stiffness without adding weight, move the 0-degree plies to the outer surfaces; [A] does not change but D₁₁ increases noticeably.
NABAK CompositePage 6 of 19
Practical Analysis of FRP Composite Laminates
Practical Analysis of Composite Laminates

5Laminate types, couplings and effective constants

Laminate typeExampleZero termsBehavior
Specially orthotropic single ply[0]ₙB, A₁₆, A₂₆, D₁₆, D₂₆Simplest; no coupling
Symmetric cross-ply[0/90]sB, A₁₆, A₂₆, D₁₆, D₂₆"Specially orthotropic"; closed-form solutions
Antisymmetric cross-ply[0/90]ₙA₁₆, A₂₆, D₁₆, D₂₆; only B₁₁ = −B₂₂Extension-bending coupling
Symmetric angle-ply[±θ]sBD₁₆ and D₂₆ non-zero; bend-twist coupling
Antisymmetric angle-ply[θ/−θ]ₙA₁₆, A₂₆, D₁₆, D₂₆; only B₁₆, B₂₆Extension-twisting coupling
Quasi-isotropic[0/±45/90]sB; A as if isotropicIn-plane stiffness independent of direction

Physical meaning of the couplings

  • Extension-bending (B): stretching an unsymmetric laminate bends it; after curing and cooling, the plate warps.
  • Extension-shear (A₁₆, A₂₆): simple tension causes shear distortion.
  • Bend-twist (D₁₆, D₂₆): bending twists the plate; in ±θ laminates it decreases with more plies but never becomes fully zero (except with special layups).

Effect of the number of plies

In antisymmetric laminates, keeping total thickness constant and increasing the number of plies (thinner, alternating plies) reduces the magnitude of B. From four to six plies onward, behavior is almost like a specially orthotropic laminate. The same trend holds for D₁₆ and D₂₆ in symmetric ±θ laminates.

Effective engineering constants of the laminate

Ex = 1/(h·a₁₁)   Ey = 1/(h·a₂₂)   Gxy = 1/(h·a₆₆)   νxy = −a₁₂/a₁₁    [a] = [A]⁻¹ (symmetric laminates)
Ex(flexural) = 12/(h³·d₁₁)    [d] = [D]⁻¹

A laminate's effective tensile modulus and effective flexural modulus are different; the flexural modulus depends on the ply sequence. This is why FRP profile property tables report the tensile and flexural moduli separately.

Key pointDefault design rule: symmetric laminate (B = 0) and balanced (A₁₆ = A₂₆ = 0). Coupling is allowed only when deliberately designed for a specific behavior (e.g. a self-adjusting blade).
NABAK CompositePage 7 of 19
Practical Analysis of FRP Composite Laminates
Practical Analysis of Composite Laminates

6Thermal and moisture effects in laminates

Temperature change and moisture absorption create "free" strains in each ply. Because plies at different angles are bonded together and cannot deform freely, internal or residual stresses arise.

{σ}ₖ = [Q̄]ₖ·( {ε} − {ᾱ}ₖ·ΔT − {β̄}ₖ·ΔM )
ᾱx = α₁m² + α₂n²    ᾱy = α₁n² + α₂m²    ᾱxy = 2(α₁ − α₂)mn

Equivalent thermal forces and moments

{N^T} = Σ ∫ [Q̄]ₖ{ᾱ}ₖ·ΔT dz     {M^T} = Σ ∫ [Q̄]ₖ{ᾱ}ₖ·ΔT·z dz
{N + N^T; M + M^T} = [ABD]·{ε⁰; κ}

Moisture effects enter in the same way by replacing α with β and ΔT with the change in moisture. In a symmetric laminate at uniform temperature, M^T is zero and the plate only changes dimensions in-plane; in an unsymmetric laminate, M^T is non-zero and the plate warps.

Residual stresses from cure

  • The laminate forms at the cure temperature (stress-free) and then cools to ambient temperature; ΔT is negative and large (e.g. 100 to 150 degrees).
  • Because α₂ is several times α₁, the 90-degree plies want to contract more and the 0-degree plies prevent it; the result is transverse tensile stress in the 90-degree plies.
  • This residual stress can use up a significant part of the transverse strength and cause matrix cracking earlier than predicted without residual stress.
  • Moisture absorption swells the matrix and offsets part of the residual thermal stress, but reduces matrix-controlled properties.

Practical application

Warping of unsymmetric laminates after cure is a simple way to determine residual stresses experimentally. Also, in designing dimensionally stable laminates (e.g. space structures), the laminate's effective expansion coefficient is designed to be near zero by choosing the angles.

Key pointDo not drop residual thermal stresses in laminate strength analysis. Without them, the onset of matrix cracking in transverse plies is predicted dangerously optimistically.
NABAK CompositePage 8 of 19
Practical Analysis of FRP Composite Laminates
Practical Analysis of Composite Laminates

7First-order shear deformation theory (FSDT)

In composites, the transverse shear moduli (G₁₃, G₂₃) are very small compared with E₁; so through-thickness shear deformation, which is negligible in metals, can be important in composite laminates. First-order shear deformation theory (Mindlin-Reissner plate theory for laminates) includes this effect.

Displacement field

u = u₀ + z·φx    v = v₀ + z·φy    w = w₀

φx and φy are independent rotations of the normal line and are no longer equal to −∂w/∂x. The normal line stays straight but is not necessarily perpendicular to the mid-plane:

γxz = φx + ∂w₀/∂x     γyz = φy + ∂w₀/∂y

Transverse shear forces and the correction factor

{Qy; Qx} = K·[[A₄₄, A₄₅], [A₄₅, A₅₅]]·{γyz; γxz}     A₄₄ = Σ Q̄₄₄⁽ᵏ⁾(zₖ − zₖ₋₁)

Because FSDT assumes constant shear strain through the thickness (whereas the real shear stress is roughly parabolic and zero at the surfaces), a shear correction factor K is introduced; the usual value is K = 5/6. For laminates, this factor depends on the layup and can be calculated by energy methods.

Comparison of CLPT and FSDT

FeatureCLPTFSDT
Primary variablesu₀, v₀, w₀ (three variables)u₀, v₀, w₀, φx, φy (five variables)
Transverse shearNeglectedConstant through the thickness with factor K
Continuity required in FEMC¹ (continuous derivative of w)C⁰ (simpler)
DeflectionLower than actualCloser to actual
Buckling load and frequencyHigher than actualCloser to actual
Range of validityThin plates (a/h > about 20–50)Thin to moderately thick

More advanced theories

Third-order shear theory (Reddy) gives a parabolic shear distribution without a correction factor; layerwise theories (Layerwise) and 3D analysis are needed for accurate interlaminar stresses, free edges and very thick laminates.

Key pointWherever the length-to-thickness ratio is less than about 20 or the E₁/G₁₃ ratio is large (carbon/epoxy, sandwich with a soft core), use FSDT or a higher theory. Under these conditions classical theory underestimates deflection and overestimates buckling; both unsafe.
NABAK CompositePage 9 of 19
Practical Analysis of FRP Composite Laminates
Practical Analysis of Composite Laminates

8Governing equations and boundary conditions of plates

The equations of motion of a composite plate are derived with the principle of virtual work (or Hamilton's principle for the dynamic case). This energy approach naturally gives both the equations and the consistent boundary conditions.

CLPT equilibrium equations

∂Nx/∂x + ∂Nxy/∂y = I₀·ü₀     ∂Nxy/∂x + ∂Ny/∂y = I₀·v̈₀
∂²Mx/∂x² + 2∂²Mxy/∂x∂y + ∂²My/∂y² + 𝒩(w₀) + q = I₀·ẅ₀ − I₂·∇²ẅ₀

𝒩(w₀) is the effect of in-plane forces (Nx∂²w/∂x² + …) needed for buckling analysis. I₀ = ρh is the translational inertia and I₂ = ρh³/12 the rotary inertia.

FSDT equations

∂Qx/∂x + ∂Qy/∂y + 𝒩(w₀) + q = I₀·ẅ₀    ∂Mx/∂x + ∂Mxy/∂y − Qx = I₂·φ̈x    ∂Mxy/∂x + ∂My/∂y − Qy = I₂·φ̈y

Boundary conditions

Edge typeCLPTFSDT
Clamped (C)u₀ = v₀ = w₀ = ∂w₀/∂n = 0u₀ = v₀ = w₀ = φn = φs = 0
Simply supported SS-1w₀ = 0, Mnn = 0, us = 0, Nnn = 0Plus φs = 0
Simply supported SS-2w₀ = 0, Mnn = 0, un = 0, Nns = 0Plus φs = 0
Free (F)All force and moment resultants zero (with the Kirchhoff effective shear force)Nnn = Nns = Mnn = Mns = Qn = 0

In composite plates, unlike isotropic plates, the in-plane edge conditions (SS-1 versus SS-2) affect deflection and buckling because of B coupling. The book stresses that "simply supported" is ambiguous for composites unless the in-plane condition is specified.

Types of analysis

  • Static: inertia terms dropped; deflection and stress under transverse load q.
  • Buckling: q = 0 and no inertia; an eigenvalue problem for the in-plane load factor.
  • Free vibration: q = 0 and harmonic response; an eigenvalue problem for natural frequencies.
  • Transient response: time integration for dynamic loads and impact.
Key pointModel the real boundary conditions of the structure accurately. In unsymmetric composite plates, the difference between SS-1 and SS-2 can noticeably change deflection and buckling load.
NABAK CompositePage 10 of 19
Practical Analysis of FRP Composite Laminates
Practical Analysis of Composite Laminates

9Bending of composite plates: Navier and Lévy solutions

Navier solution

For an a×b rectangular plate with simple supports, displacements are assumed as double Fourier series that automatically satisfy the boundary conditions. The Navier solution is exact only for specific layups:

  • Specially orthotropic (symmetric cross-ply), simply supported
  • Antisymmetric cross-ply with SS-1
  • Antisymmetric angle-ply with SS-2
w₀ = Σ Σ Wmn·sin(mπx/a)·sin(nπy/b)
Wmn = Qmn / { π⁴·[ D₁₁(m/a)⁴ + 2(D₁₂+2D₆₆)(m/a)²(n/b)² + D₂₂(n/b)⁴ ] }    (specially orthotropic, CLPT)
uniform load: Qmn = 16q₀/(π²mn), m, n odd

The series converges quickly for deflection but needs more terms for moments and especially transverse shear stresses.

Lévy solution

If two opposite edges are simply supported and the other two have any condition (clamped, free, simply supported), the solution is assumed as a single series with an unknown function in the other direction, and the problem becomes an ordinary differential equation. The Lévy solution is valuable for assessing the effect of boundary conditions and verifying finite element results.

Cylindrical bending

A plate that is very long in one direction under a load that is constant in that direction behaves like a strip or wide beam. This problem has an exact 3D elasticity solution (Pagano) and is the classic benchmark for assessing the accuracy of CLPT and FSDT.

Trends in the results

  • The CLPT non-dimensional deflection is independent of a/h; FSDT shows that deflection increases as a/h decreases (thicker plate).
  • An antisymmetric laminate with few plies, because of B coupling, deflects more than a symmetric laminate of the same weight; this difference disappears as the number of plies increases.
  • Increasing E₁/E₂ intensifies the transverse shear effect.
  • Transverse shear stresses are recovered more accurately from the 3D equilibrium equations by integrating through the thickness than from the constitutive relations.
Key pointNavier and Lévy solutions are verification tools: before trusting a finite element model of a complex structure, test the same model on a simple plate with an analytical solution.
NABAK CompositePage 11 of 19
Practical Analysis of FRP Composite Laminates
Practical Analysis of Composite Laminates

10Buckling of composite plates

Because of composites' high strength-to-stiffness ratio and thin walls, buckling is often the governing design mode for composite plates and profiles.

Critical load of a specially orthotropic plate (CLPT)

Under biaxial compression Nx = N₀ and Ny = k·N₀ with simple supports:

N₀ = π²·[ D₁₁m⁴ + 2(D₁₂+2D₆₆)m²n²s² + D₂₂n⁴s⁴ ] / ( a²·(m² + k·s²·n²) )    s = a/b

The critical load is the minimum of this expression over all values of m and n. For uniaxial compression, n = 1 and the number of half-waves m in the load direction depends on the aspect ratio and the stiffness ratios; longer plates buckle with several half-waves.

Factors affecting buckling

FactorEffect
Ply sequence±45 plies on the outside raise D₆₆ and D₁₂; effective for buckling
B coupling (antisymmetric laminate)Reduces buckling load; decreases as the number of plies increases
D₁₆ and D₂₆ (bend-twist)Reduce buckling load; ignoring them is unsafe
Shear deformation (FSDT)Reduces buckling load in thick plates and sandwiches
Boundary conditionsClamped carries more load than simply supported
Initial imperfectionReduces actual capacity; post-buckling and nonlinear behavior

Shear and combined buckling

Shear load Nxy has no closed-form solution and is calculated with approximate methods (Ritz, Galerkin) or finite elements. In ±θ laminates, the direction of shear (positive or negative) gives a different buckling load.

Post-buckling

Like metal plates, composite plates still have capacity after buckling, but failure may occur earlier because of large bending stresses and delamination in the post-buckling regime; post-buckling design of composites requires nonlinear analysis and caution.

Note for FRP profilesThe flanges and webs of pultruded I, H and channel profiles are long plates with semi-clamped or free edges; local buckling of the compression flange and lateral-torsional buckling of the beam usually occur before the material strength is reached.
Key pointIn designing composite plates in compression, check buckling first; material strength is often the second constraint. Increasing thickness or using a sandwich is the most effective way to raise the buckling load.
NABAK CompositePage 12 of 19
Practical Analysis of FRP Composite Laminates
Practical Analysis of Composite Laminates

11Free vibration of composite plates

The natural frequencies and mode shapes of a composite plate matter for avoiding resonance and for design against dynamic and acoustic loads. The response is assumed harmonic, w = W·e^(iωt), and the equations become an eigenvalue problem.

Natural frequency of a simply supported specially orthotropic plate (CLPT)

ω²mn = π⁴·[ D₁₁(m/a)⁴ + 2(D₁₂+2D₆₆)(m/a)²(n/b)² + D₂₂(n/b)⁴ ] / ( I₀ + I₂·π²[(m/a)² + (n/b)²] )

Neglecting rotary inertia (I₂), the denominator equals I₀ = ρh. The similarity of the numerator of this relation to the buckling load and deflection shows that all three problems are controlled by the same combination of bending stiffnesses.

Non-dimensionalization

ω̄ = ω·(b²/h)·√(ρ/E₂)

The non-dimensional frequency allows laminates and theories to be compared independently of absolute dimensions. The book gives many tables and plots of the effect of aspect ratio, a/h, E₁/E₂, number of plies and fiber angle on the fundamental frequency.

Important trends

  • CLPT overestimates frequencies; the error is larger for higher modes and thicker plates, because shorter wavelengths increase the shear contribution.
  • B coupling in antisymmetric laminates with few plies lowers the frequency.
  • The optimal fiber angle for maximizing the fundamental frequency depends on the plate aspect ratio; for a square plate, ±45 laminates usually have the highest frequency.
  • In-plane tensile force raises the frequency and compressive force lowers it; at the critical buckling load, the fundamental frequency reaches zero.

Damping

The polymer matrix gives composites several times the damping of metals; damping is higher in the transverse and shear directions. By designing the ply angles or adding viscoelastic layers, structural damping can be increased.

Key pointComposites' high stiffness-to-mass ratio raises natural frequencies; an important advantage for rotating, automotive and aircraft structures. But higher modes must be analyzed with FSDT or finite elements.
NABAK CompositePage 13 of 19
Practical Analysis of FRP Composite Laminates
Practical Analysis of Composite Laminates

12Laminated composite beams

A composite beam can be thought of as a narrow plate. The book shows how laminate stiffnesses are converted into beam stiffness and how Euler-Bernoulli and Timoshenko theories are applied to laminated beams.

Effective bending stiffness

In a narrow beam, My and Mxy are assumed zero on the free edges (not κy and κxy). The bending compliance matrix is therefore used:

Mx = (b / d*₁₁)·κx     E_xx^b = 12 / (h³·d*₁₁)     [d*] = [D]⁻¹ (symmetric)

Using D₁₁ instead of 1/d*₁₁ overestimates stiffness (the Poisson effect and twisting coupling are ignored). In an unsymmetric laminate, the full ABD inverse is used.

Euler-Bernoulli theory

E_xx^b·I·d⁴w/dx⁴ = q(x)

All classical beam deflection formulas (cantilever, simply supported, etc.) can be used by replacing EI with the laminate's effective bending stiffness.

Timoshenko theory

w_total = w_bending + w_shear     e.g. simply supported, uniform load: w_max = 5qL⁴/(384·EI) + qL²/(8·K·G·A)

Because the E/G ratio is large in composites, the shear deflection contribution is significant in short beams or those with a low span-to-depth ratio. Three-point bending tests at several spans are a practical way to determine the effective E and G together.

Thin-walled beams

In I, box and channel sections, each part (flange, web) is a separate laminate. The section's bending stiffness is calculated by summing the parts' contributions (axial stiffness of each part times the square of its distance from the neutral axis). Torsion, section warping and the shear center in open composite sections also depend on the ply sequence.

Beam vibration and buckling

The natural frequency and Euler buckling load of a composite beam are obtained with the same classical relations and the effective bending stiffness; the shear effect reduces both.

Note for FRP profilesIn pultruded beams, deflection usually governs design. With a flexural modulus of about 20 to 30 GPa and a shear modulus of about 3 to 4 GPa, shear deflection is a noticeable share in short spans and must be calculated with Timoshenko theory.
Key pointFor a composite beam, never put the tensile modulus in the deflection formula; calculate the effective bending stiffness (dependent on ply sequence) and the shear contribution separately.
NABAK CompositePage 14 of 19
Practical Analysis of FRP Composite Laminates
Practical Analysis of Composite Laminates

13Finite element analysis of laminates

Analytical solutions exist only for simple geometries, layups and boundary conditions. Real composite structures (with holes, stiffeners, variable thickness and complex loads) are analyzed with the finite element method. The book describes finite element formulations for both theories.

CLPT elements

Because the strain energy contains the second derivative of w, C¹ continuity (continuity of w and its slopes) is required. Rectangular elements with Hermite interpolation (such as nonconforming or conforming elements with degrees of freedom w, ∂w/∂x, ∂w/∂y and ∂²w/∂x∂y) are used. Building C¹ elements for arbitrary geometries is difficult.

FSDT elements

FSDT requires only C⁰ continuity; all five variables are interpolated with Lagrange functions (linear or quadratic). This simplicity has made FSDT the basis of composite shell elements in commercial software.

Shear locking

In thin plates, FSDT elements with full integration cannot satisfy the condition of near-zero shear strain and become overly stiff. Remedies:

  • Reduced or selective integration: the shear terms are integrated with fewer Gauss points.
  • Higher-order elements (eight- or nine-node).
  • Assumed strain field or mixed formulations.

Reduced integration may produce zero-energy (hourglass) modes that must be controlled.

Practical modeling notes

  • Define the reference direction of ply angles in each element; orientation errors are the most common mistake in composite models.
  • Check mesh convergence, especially for stresses (which converge more slowly than displacements).
  • For interlaminar stresses and free edges, shell elements are not enough; a 3D or layerwise model is needed.
  • Verify against a Navier or Lévy solution for a simple problem.
  • Geometrically nonlinear analysis for large deflections and post-buckling.
Key pointFinite element software will deliver any number; its correctness depends on the choice of theory, element type, ply orientations and boundary conditions. Knowing the theory behind the element is a condition for using it with confidence.
NABAK CompositePage 15 of 19
Practical Analysis of FRP Composite Laminates
Practical Analysis of Composite Laminates

14Failure and progressive damage analysis

After calculating the stresses, the designer's main question is: at what load does the composite laminate fail? The book presents lamina failure criteria and laminate failure analysis methods in a practical way.

Basic lamina strengths

X_t and X_c (longitudinal tension and compression), Y_t and Y_c (transverse tension and compression) and S (in-plane shear). For analysis with FSDT, transverse shear strengths are also needed.

Failure criteria

CriterionTypeFeature
Maximum stress / maximum strainNon-interactiveSimple; identifies the failure mode (fiber, matrix, shear)
Tsai-HillQuadratic interactiveOne strength for tension and compression in each direction
Tsai-WuTensor polynomialDifference between tension and compression; interaction coefficient F₁₂
HashinMechanism-basedSeparates fiber and matrix failure in tension and compression
Tsai–Wu: F₁σ₁ + F₂σ₂ + F₁₁σ₁² + F₂₂σ₂² + F₆₆τ₁₂² + 2F₁₂σ₁σ₂ = 1

The safety factor or "strength ratio" R is obtained by replacing σ with R·σ and solving the quadratic equation; R > 1 means the ply is intact.

First-ply failure and progressive failure

  1. Calculate each ply's stress in material axes under unit load.
  2. Find the lowest R among the plies: the first-ply failure (FPF) load.
  3. Reduce the properties of the damaged ply according to the failure mode: matrix failure → reduce E₂ and G₁₂; fiber failure → reduce E₁ (and other properties).
  4. Recalculate ABD and redistribute stress; repeat until last-ply failure (LPF).

The book also implements this procedure for plates in bending with finite elements: damage starts at high-stress points and spreads gradually, and the load-deflection curve becomes nonlinear.

Interlaminar stresses and delamination

At free edges, holes, ply drops and joints, the interlaminar stresses σz, τxz and τyz become large and can initiate delamination. CLPT does not give these stresses; recovery from the equilibrium equations or 3D analysis is needed. Simple criteria such as comparison with interlaminar strength, or fracture mechanics (energy release rate), are used.

Key pointAlways apply the failure criterion in material axes and with residual thermal stresses. First-ply failure is usually matrix cracking, not collapse; but in a corrosive environment or under fatigue, that crack is where damage begins.
NABAK CompositePage 16 of 19
Practical Analysis of FRP Composite Laminates
Practical Analysis of Composite Laminates

15Practical design of laminates and composite structures

The practical part of the book (drawing on Miravete's industrial experience) links analysis to the design process: selecting material, layup, dimensions and details, with criteria for stiffness, strength, stability, weight and cost.

Design steps

  1. Define loads, boundary conditions, environment (temperature, moisture, chemicals) and requirements (deflection, frequency, weight).
  2. Select the material system and manufacturing method (lay-up, RTM, filament winding, pultrusion), which limits the possible fiber arrangements.
  3. Preliminary layup design with carpet plots (carpet plots): modulus and strength of 0/±45/90 laminates as a function of the percentage in each direction.
  4. Analysis with CLPT/FSDT or finite elements; check deflection, buckling, vibration and failure.
  5. Details: holes, joints, ply drops, stiffeners.
  6. Apply environmental knockdown factors and a safety factor; test coupons and components.

Layup rules

  • Symmetric and balanced; at least about 10% of plies in each of the 0, ±45 and 90 directions.
  • Don't stack more than four same-orientation plies together (reduces interlaminar stress and cracking).
  • ±45 plies on the outer surfaces for resistance to impact, buckling and shear.
  • Angle change between adjacent plies at most about 45 to 60 degrees.
  • Gradual ply drops with a gentle taper.

Stress concentration at holes

K_t∞ = 1 + √( 2(√(E₁/E₂) − ν₁₂) + E₁/G₁₂ )    (infinite orthotropic plate, Lekhnitskii)

For an isotropic material K_t = 3, but for a unidirectional carbon/epoxy laminate it can reach about 6 to 8; a quasi-isotropic laminate has a value close to 3. But because composites tolerate local damage, point stress or average stress criteria (Whitney-Nuismer) are used to predict open-hole strength.

Joints and sandwich structures

Bolted joints (failure modes: bearing, net tension, shear-out) and bonded joints (shear stress concentration at the ends of the overlap) are common weak points of a structure. Sandwich structures with composite skins and a light core give very high bending stiffness at low weight, but core shear deformation and face wrinkling must be checked.

Key pointMost failures in composite structures occur in details: holes, joints and ply drops, not in the uniform laminate region. Take detail design more seriously than overall design.
NABAK CompositePage 17 of 19
Practical Analysis of FRP Composite Laminates
Practical Analysis of Composite Laminates

16Conclusions and frequently asked questions

Ten golden rules of laminate analysis

  1. All analyses start from the ply's [Q] matrix and continue with [Q̄] in structural axes.
  2. [A] does not depend on ply sequence; [D] depends on it strongly.
  3. A symmetric, balanced laminate eliminates unwanted couplings.
  4. B coupling and D₁₆/D₂₆ reduce stiffness, buckling load and frequency; they decrease as the number of plies increases.
  5. Include residual thermal stresses in strength.
  6. CLPT for thin plates; FSDT for moderately thick plates and materials with large E₁/G₁₃.
  7. CLPT underestimates deflection and overestimates buckling and frequency.
  8. In a composite beam, calculate the effective bending stiffness from the inverse of D and the shear deflection separately.
  9. In finite elements, control shear locking and ply orientations, and verify the model against an analytical solution.
  10. Failure often starts at details (holes, joints, edges) and from interlaminar stresses.

Application for FRP profile manufacturers

Every pultruded profile can be seen as a set of laminated plates (flanges and webs) made of unidirectional roving plies and mat or fabric. With the tools in this book, each wall's properties can be calculated from the layup, the beam's bending and shear stiffness determined, local buckling of flanges and webs checked and strength assessed with a failure criterion; that is, from the data sheet to a reliable structural design.

Frequently asked questions

What is the difference between classical theory and first-order shear deformation theory? Classical theory ignores transverse shear and suits thin laminates; FSDT, with two independent rotations and a shear correction factor, gives more accurate results for thicker laminates.

When is the Navier solution valid for a composite plate? For simply supported rectangular plates with symmetric cross-ply, antisymmetric cross-ply (SS-1) and antisymmetric angle-ply (SS-2) layups.

Why does an antisymmetric laminate have lower stiffness? Because of extension-bending coupling, which increases deflection and reduces buckling load and frequency; this effect decreases as the number of plies increases.

When is a 3D model needed? For accurate interlaminar stresses at edges, holes, ply drops, joints and in very thick laminates.

NABAK CompositePage 18 of 19
Practical Analysis of FRP Composite Laminates
Practical Analysis of Composite Laminates

17Glossary of laminate analysis terms

English termMeaningShort explanation
Lamina / PlySingle plyBasic unit of the laminate
Laminate / Stacking sequenceLaminate / stacking sequenceSet and order of plies
Specially orthotropicSpecially orthotropicNo coupling at all
Cross-ply / Angle-plyCross-ply / angle-ply0/90 or ±θ
Symmetric / AntisymmetricSymmetric / antisymmetricRelative to the mid-plane
BalancedBalancedA₁₆ = A₂₆ = 0
CLPTClassical laminated plate theoryKirchhoff assumptions
FSDTFirst-order shear deformation theoryIndependent rotations; constant shear
Shear correction factorShear correction factorUsually 5/6
Extension–bending couplingExtension-bending couplingB matrix
Bending–twisting couplingBend-twist couplingD₁₆ and D₂₆
Navier / Lévy solutionNavier / Lévy solutionAnalytical Fourier series solution
Cylindrical bendingCylindrical bendingLong plate; benchmark problem
Critical buckling loadCritical buckling loadInstability load
Natural frequency / Mode shapeNatural frequency / mode shapeFree vibration
Rotary inertiaRotary inertiaI₂ term
Shear lockingShear lockingSpurious stiffness of FSDT elements
Reduced integrationReduced integrationRemoving locking
First-ply failureFirst-ply failureDamage initiation
Progressive failureProgressive failureProperty reduction and repeated analysis
Interlaminar stressInterlaminar stressCause of delamination
Carpet plotCarpet plotPreliminary layup design tool

Related keywords: laminate analysis, composite laminates, composite plates, composite analysis, FRP composites, classical lamination theory, first-order shear deformation theory, ABD matrix, buckling and vibration of composite plates, composite beams, finite elements, composite design, FRP profiles, NABAK Composite.

NABAK CompositePage 19 of 19