Mechanics of Composite Materials and FRP Composites
Mechanics of Composite Materials

Mechanics of Composite Materials

Mechanics of Composite Materials: A Comprehensive Book Summary

A complete guide to the mechanics of FRP composites: lamina macromechanics and micromechanics, restrictions on engineering constants, failure criteria, classical lamination theory, interlaminar stresses, bending, buckling and vibration of plates, fatigue and damage tolerance, joints and the design of composite structures

Author of the original book: Robert M. Jones
Publisher: Taylor & Francis — field: mechanics and design of composite materials
Prepared for: NABAK Composite

About this book

Robert Jones's book is one of the most classic and most cited references on the mechanics of composite materials in the world, and several generations of aerospace, mechanical and civil engineers have been trained on it. Its structure moves from the "lamina" to the "laminate" and then to "structures and design", and at each stage it distinguishes between the macromechanical approach (the apparent behavior of the material) and the micromechanical approach (the interaction of fiber and matrix). Its distinctive features are a careful discussion of the physical restrictions on engineering constants, an experimental comparison of failure criteria, free-edge interlaminar stresses and the philosophy of composite structural design.

How to use this summary

  • Orange "Key point" boxes give the most important engineering conclusion of each chapter.
  • Gold "Note" boxes show how the material applies to designing and producing FRP composite products such as profiles, panels and tanks.
  • Direction 1 is along the fibers, 2 is perpendicular to the fibers in the plane and 3 is through the thickness; X, Y and S are the longitudinal, transverse and shear strengths of the lamina.
  • Sample figures are given to convey scale and are no substitute for test data.
NABAK CompositePage 1 of 18
Mechanics of Composite Materials and FRP Composites
Mechanics of Composite Materials

Table of Contents

  1. 1Introduction: composite materials, classification and terminology
  2. 2Lamina macromechanics: stress-strain relations
  3. 3Restrictions on engineering constants, transformation and invariants
  4. 4Lamina strength and biaxial failure criteria
  5. 5Micromechanics of stiffness
  6. 6Micromechanics of strength
  7. 7Laminate macromechanics: classical theory
  8. 8Special laminate cases and stiffness behavior
  9. 9Laminate strength and hygrothermal effects
  10. 10Interlaminar stresses and the free-edge effect
  11. 11Bending, buckling and vibration of laminated plates
  12. 12Fatigue, damage tolerance and fracture mechanics
  13. 13Transverse shear, environmental effects and joints
  14. 14Introduction to composite structural design
  15. 15Conclusions and frequently asked questions
  16. 16Glossary of composite mechanics terms
The book's main message in one sentenceA composite must be seen as both a "material" and a "structure" at once: lamina properties come from fiber and matrix, laminate behavior from the ply sequence and structural safety from understanding failure and damage mechanisms; and all three must be considered together in design.
NABAK CompositePage 2 of 18
Mechanics of Composite Materials and FRP Composites
Mechanics of Composite Materials

1Introduction: composite materials, classification and terminology

A composite material is made by combining two or more materials on a macroscopic scale to obtain better properties than the constituents: strength, stiffness, low weight, corrosion resistance, wear resistance, insulation, fatigue life and special thermal or acoustic behavior. The book introduces four main families:

FamilyDescriptionExample
Fiber compositeFibers in a matrixFRP composites: glass/polyester, carbon/epoxy
Laminated compositeLayers of different materialsBimetals, safety glass, FRP laminates, sandwiches
Particulate compositeParticles in a matrixConcrete, cermets, filled polymers
CombinedCombination of the aboveFiber laminate with filled matrix

Why fibers?

Because of flaws, a bulk material has far lower strength than its theoretical strength. In thin fiber form, flaw size is limited and strength increases several-fold (as with glass, which as a fresh fiber has a strength of several gigapascals). The matrix holds the fibers together, transfers load and protects the fibers from the environment and damage.

Basic terms

  • Lamina (ply): a flat or curved layer of unidirectional or woven fibers in a matrix.
  • Laminate: several bonded plies with different orientations.
  • Macromechanics: study of material behavior assuming homogeneity and using average apparent properties.
  • Micromechanics: study of fiber–matrix interaction to predict apparent properties.
  • Homogeneous / heterogeneous, isotropic / anisotropic: a material may be heterogeneous on the micro scale but "apparently homogeneous" and anisotropic on the structural scale.

Applications and challenges

The book reviews aerospace, automotive, sporting, marine and industrial applications and stresses that the composite advantage is realized only when design uses the material "in the right amount and in the right direction". Main challenges: anisotropy, couplings, interlaminar stresses, sensitivity to impact and environment, and manufacturing cost.

Key pointThe distinction between macromechanics and micromechanics is the backbone of the book: for structural design macromechanics is usually enough, but micromechanics is needed to select and improve the material and to understand failure.
NABAK CompositePage 3 of 18
Mechanics of Composite Materials and FRP Composites
Mechanics of Composite Materials

2Lamina macromechanics: stress-strain relations

The book starts from the generalized Hooke's law for an anisotropic material and arrives at simpler cases by adding planes of symmetry. The conceptual point is that the number of independent constants is a "material property" and determines the number of tests needed.

σᵢ = Cᵢⱼ·εⱼ    Cᵢⱼ = Cⱼᵢ    → 21 (anisotropic), 13 (monoclinic), 9 (orthotropic), 5 (transversely isotropic), 2 (isotropic)

Orthotropic material in terms of engineering constants

ε₁ = σ₁/E₁ − ν₂₁σ₂/E₂ − ν₃₁σ₃/E₃    γ₂₃ = τ₂₃/G₂₃    …    νᵢⱼ/Eᵢ = νⱼᵢ/Eⱼ

Poisson's ratio νᵢⱼ is the ratio of the transverse strain in direction j to the strain in the loading direction i. Symmetry of the compliance matrix requires the reciprocal relation above; this relation is an important check on laboratory data.

Plane stress state

[Q] = [[E₁/(1−ν₁₂ν₂₁), ν₁₂E₂/(1−ν₁₂ν₂₁), 0], [ν₁₂E₂/(1−ν₁₂ν₂₁), E₂/(1−ν₁₂ν₂₁), 0], [0, 0, G₁₂]]

For thin plies, σ₃ = τ₂₃ = τ₃₁ = 0 is assumed and four constants E₁, E₂, ν₁₂ and G₁₂ fully describe the in-plane behavior of the lamina.

Lamina with arbitrary orientation

In rotated axes, the stiffness matrix [Q̄] has six non-zero components, and Q̄₁₆ and Q̄₂₆ represent shear-extension coupling. The book calls a lamina whose principal axes coincide with the loading axes "specially orthotropic", and otherwise "generally orthotropic"; the latter has apparently anisotropic behavior.

Coupling coefficients and Chentsov coefficients

In a generally orthotropic lamina, besides the usual engineering constants, coefficients of mutual influence (shear strain caused by normal stress and vice versa) and Chentsov coefficients (interaction of shear strains) are defined. These coefficients show up in tests on off-axis specimens.

Key pointA composite lamina is simple in material axes and complex in rotated axes. Always understand the behavior in material axes and transfer it to the load axes for the structure by coordinate transformation.
NABAK CompositePage 4 of 18
Mechanics of Composite Materials and FRP Composites
Mechanics of Composite Materials

3Restrictions on engineering constants, transformation and invariants

Physical restrictions on engineering constants

One of the hallmark sections of Jones's book: because strain energy must be positive, the stiffness and compliance matrices must be positive definite. The result:

E₁, E₂, E₃, G₁₂, G₂₃, G₃₁ > 0    |ν₁₂| < (E₁/E₂)^½    |ν₂₃| < (E₂/E₃)^½    |ν₁₃| < (E₁/E₃)^½
Δ = 1 − ν₁₂ν₂₁ − ν₂₃ν₃₂ − ν₃₁ν₁₃ − 2ν₂₁ν₃₂ν₁₃ > 0

Unlike isotropic materials, where ν must lie between −1 and 0.5, in an anisotropic material Poisson's ratio can exceed 0.5 (e.g. in ±25 degree laminates νxy can exceed 1) without violating the laws of physics. These restrictions are a tool for checking test data and the output of micromechanics models.

Coordinate transformation

Q̄₁₁ = Q₁₁cos⁴θ + 2(Q₁₂+2Q₆₆)sin²θcos²θ + Q₂₂sin⁴θ
1/Ex = cos⁴θ/E₁ + (1/G₁₂ − 2ν₁₂/E₁)·sin²θcos²θ + sin⁴θ/E₂

The book shows that Ex does not necessarily lie between E₁ and E₂: if G₁₂ is large or small enough, Ex at an intermediate angle may be larger or smaller than both.

Stiffness invariants (Tsai-Pagano)

U₁ = (3Q₁₁+3Q₂₂+2Q₁₂+4Q₆₆)/8   U₂ = (Q₁₁−Q₂₂)/2   U₃ = (Q₁₁+Q₂₂−2Q₁₂−4Q₆₆)/8
U₄ = (Q₁₁+Q₂₂+6Q₁₂−4Q₆₆)/8   U₅ = (Q₁₁+Q₂₂−2Q₁₂+4Q₆₆)/8
Q̄₁₁ = U₁ + U₂cos2θ + U₃cos4θ    Q̄₁₂ = U₄ − U₃cos4θ    Q̄₆₆ = U₅ − U₃cos4θ

U₁, U₄ and U₅ are independent of angle; they represent the material's "stiffness capacity", and the angle only distributes this capacity among directions. In a quasi-isotropic laminate, A₁₁ = U₁h, A₁₂ = U₄h and A₆₆ = U₅h.

Key pointThe invariants show that no layup can raise stiffness in all directions beyond what the material offers; it can only be directed. A quasi-isotropic laminate gives the average stiffness in all directions.
NABAK CompositePage 5 of 18
Mechanics of Composite Materials and FRP Composites
Mechanics of Composite Materials

4Lamina strength and biaxial failure criteria

An orthotropic lamina has five basic strengths: X_t and X_c (longitudinal tension and compression), Y_t and Y_c (transverse tension and compression) and S (shear). The book stresses that these strengths are meaningful only in material axes and that shear strength, unlike normal strengths, does not depend on the sign of the shear stress; but in rotated axes, the sign of the shear matters.

Failure criteria

CriterionRelationFeature
Maximum stressσ₁ < X, σ₂ < Y, |τ₁₂| < SThree separate criteria; identifies the failure mode
Maximum strainε₁ < X_ε, ε₂ < Y_ε, |γ₁₂| < S_γPoisson effect; close to maximum stress
Tsai-Hillσ₁²/X² − σ₁σ₂/X² + σ₂²/Y² + τ₁₂²/S² = 1Interactive; X and Y chosen according to stress sign
HoffmanLinear terms for the tension-compression differenceGeneralization of Tsai-Hill
Tsai-WuFᵢσᵢ + Fᵢⱼσᵢσⱼ = 1Tensor polynomial; F₁₂ requires a biaxial test
Hoffman: σ₁²/(XtXc) − σ₁σ₂/(XtXc) + σ₂²/(YtYc) + (1/Xt − 1/Xc)σ₁ + (1/Yt − 1/Yc)σ₂ + τ₁₂²/S² = 1

Comparison with experiment

The book compares data from off-axis uniaxial glass/epoxy specimens with the criteria. Result: the maximum stress and maximum strain criteria give a jagged curve with "cusps" and overestimate strength at intermediate angles (about 10 to 45 degrees), while Tsai-Hill agrees better with the data. The reason: stresses do interact in real failure.

Choosing the interaction coefficient F₁₂

F₁₂ requires a biaxial test, which is difficult, and the result is very sensitive to its accuracy. The stability condition F₁₁F₂₂ − F₁₂² > 0 must hold for the failure surface to be closed (ellipsoidal). A common approximation is F₁₂ ≈ −½√(F₁₁F₂₂).

Key pointMacromechanical failure criteria are engineering tools, not physical laws; their accuracy depends on the quality of the five basic strengths. For design, combine an interactive criterion (Tsai-Hill or Tsai-Wu) with a check of the failure mode (maximum stress).
NABAK CompositePage 6 of 18
Mechanics of Composite Materials and FRP Composites
Mechanics of Composite Materials

5Micromechanics of stiffness

The book compares three approaches for predicting the engineering constants of a lamina from fiber and matrix properties: mechanics of materials, elasticity and semi-empirical.

Mechanics of materials approach

E₁ = Ef·Vf + Em·Vm    ν₁₂ = νf·Vf + νm·Vm    1/E₂ = Vf/Ef + Vm/Em    1/G₁₂ = Vf/Gf + Vm/Gm

E₁ and ν₁₂ are accurate; E₂ and G₁₂ are underestimated, because fibers and matrix are not actually in pure series and the matrix between fibers is simultaneously constrained.

Elasticity approach

  • Bounding (energy) principles: the minimum potential energy principle gives an upper bound and the minimum complementary energy principle a lower bound. For E₂ and G₁₂ these bounds are far apart and of limited direct use.
  • Exact solutions for regular arrays: square or hexagonal fiber arrays; results are sensitive to the array.
  • Tsai's model with a contiguity factor: combining the two limiting cases of "isolated fibers" (C = 0) and "fibers in full contact" (C = 1). C increases with Vf and lies between these two for real data.

Halpin-Tsai equations

M/Mm = (1 + ξηVf)/(1 − ηVf)    η = (Mf/Mm − 1)/(Mf/Mm + ξ)

This relation is a simple interpolation of complex elasticity solutions. ξ depends on geometry, fiber arrangement and load type (about 2 for E₂ with circular fibers in a square array and about 1 for G₁₂). At high Vf, η tends toward 1 and the results become more sensitive.

Effect of volume fraction and voids

As Vf increases, E₁ rises linearly and E₂ and G₁₂ rise nonlinearly and at an accelerating rate. The theoretical maximum Vf for circular fibers is about 0.91 in a hexagonal array and about 0.785 in a square array; in practice 0.5 to 0.7. Voids sharply reduce matrix-controlled properties.

NoteThe book shows that micromechanics predictions for E₂ and G₁₂ are of the same order as the scatter in experimental data; micromechanics is therefore mainly for "understanding trends and selecting materials", and final design must use tested lamina properties.
Key pointFibers control longitudinal properties and the matrix controls transverse and shear properties. Increasing Vf raises all stiffnesses, but beyond about 0.65 to 0.7, incomplete wet-out and voids reduce transverse properties.
NABAK CompositePage 7 of 18
Mechanics of Composite Materials and FRP Composites
Mechanics of Composite Materials

6Micromechanics of strength

Longitudinal tensile strength

The book examines the common FRP composite case in which the fiber failure strain is less than the matrix's:

X_t = σ_fu·Vf + σ_m*·(1 − Vf)    (Vf > V_min)
V_min = (σ_mu − σ_m*) / (σ_fu + σ_mu − σ_m*)    V_crit = (σ_mu − σ_m*) / (σ_fu − σ_m*)

σ_m* is the matrix stress at the fiber failure strain. Below V_min, when the fibers break the matrix still carries the load and the fibers effectively behave like holes. For the composite to be stronger than the matrix, Vf must exceed V_crit. For typical FRP these values are very small and are always satisfied.

Longitudinal compressive strength (Rosen model)

In compression, fibers behave like slender columns on an elastic foundation of matrix:

extension mode: σ_c ≈ 2Vf·√(Vf·Em·Ef / (3(1−Vf)))    shear mode: σ_c ≈ Gm/(1 − Vf)

At typical Vf, the shear mode (in-phase buckling of the fibers) governs. Theoretical predictions are usually far higher than real values; reasons: initial fiber misalignment, nonlinear matrix behavior, interface debonding and kink band formation.

Transverse and shear strength

Stiff fibers concentrate strain in the matrix between fibers. The strain magnification factor grows with Vf and the Ef/Em ratio; as a result, the transverse strength of the lamina may be lower than that of the neat matrix. Interface adhesion, voids and residual thermal stresses play a decisive role.

Statistical nature of strength

Fiber strength has large scatter and decreases with length. In a composite, broken fibers pick up load again over a short length through matrix shear; this "ineffective length" makes the strength of a fiber bundle in a composite higher than that of a dry bundle.

Key pointStrength micromechanics is more qualitative than quantitative; its main value is explaining why: why compressive strength is lower than tensile (misalignment), why transverse strength is low (strain concentration) and why interface quality is vital.
NABAK CompositePage 8 of 18
Mechanics of Composite Materials and FRP Composites
Mechanics of Composite Materials

7Laminate macromechanics: classical theory

Classical laminate theory (CLT) builds the behavior of a ply stack from the ply properties and their sequence. Assumptions: plies are perfectly bonded and very thin, the Kirchhoff hypothesis (a normal line stays straight and normal), plane stress in each ply and linear elastic behavior.

{ε} = {ε⁰} + z{κ}     {σ}ₖ = [Q̄]ₖ({ε⁰} + z{κ})
{N; M} = [[A, B], [B, D]]·{ε⁰; κ}    Aᵢⱼ = Σ Q̄ᵢⱼ(zₖ−zₖ₋₁), Bᵢⱼ = ½Σ Q̄ᵢⱼ(zₖ²−zₖ₋₁²), Dᵢⱼ = ⅓Σ Q̄ᵢⱼ(zₖ³−zₖ₋₁³)

Meaning of the matrices

  • A (extensional stiffness): relates in-plane forces to mid-plane strains; independent of ply sequence.
  • B (coupling stiffness): relates in-plane force to bending and twisting; arises from asymmetry.
  • D (bending stiffness): relates moments to curvatures; strongly dependent on ply positions.

Inverse of the stiffness matrix

{ε⁰; κ} = [[A′, B′], [C′, D′]]·{N; M}

The book gives closed-form partial inversion relations (A′ = A* − B*D*⁻¹C*, etc.). For a symmetric laminate, the inverse simplifies to [A]⁻¹ and [D]⁻¹.

Analysis procedure

  1. Calculate Q for each ply, transform to Q̄.
  2. Calculate A, B, D and their inverse.
  3. Calculate ε⁰ and κ from the loads N and M.
  4. Strain and stress in each ply in x-y axes, then in material axes.
  5. Apply the failure criterion to each ply.
NoteCLT is very accurate away from edges and for thin laminates; but it assumes zero interlaminar stresses, which is wrong at edges and holes (chapter 10).
Key pointStrain through the laminate thickness is linear and continuous, but stress, because of the different Q̄ of the plies, is piecewise and discontinuous. The maximum stress may occur in an inner ply rather than at the surface.
NABAK CompositePage 9 of 18
Mechanics of Composite Materials and FRP Composites
Mechanics of Composite Materials

8Special laminate cases and stiffness behavior

The book classifies laminates by the zero terms of the ABD matrix and examines the behavior of each class with plots of stiffness against number of plies and angle.

ClassExampleZero termsCharacteristic behavior
Single isotropic or specially orthotropic ply[0]B, 16 and 26 couplingsSimplest
Symmetric unidirectional[θ]ₙBShear-extension and bend-twist coupling
Symmetric cross-ply[0/90/0]B, A₁₆, A₂₆, D₁₆, D₂₆Specially orthotropic
Symmetric angle-ply[+θ/−θ/+θ]B, A₁₆, A₂₆ (with odd plies, not fully)D₁₆, D₂₆ decrease as plies increase
Antisymmetric cross-ply[0/90]ₙAll except B₁₁ = −B₂₂Extension-bending coupling
Antisymmetric angle-ply[+θ/−θ]ₙAll except B₁₆, B₂₆Extension-twisting coupling
Quasi-isotropic[0/±60]s, [0/±45/90]sIsotropic AIn-plane stiffness independent of direction

Important results

  • In an antisymmetric cross-ply laminate of constant thickness, B₁₁ decreases with 1/N (N the number of plies); with several plies, the coupling almost disappears.
  • In an antisymmetric angle-ply laminate, too, B₁₆ and B₂₆ drop rapidly as the number of plies increases.
  • In a symmetric angle-ply laminate, D₁₆ and D₂₆ decrease as plies increase but do not become zero.
  • A quasi-isotropic laminate is not isotropic in bending; D depends on the ply sequence.

Effective engineering constants of the laminate

Ex = 1/(h·a₁₁)   Ey = 1/(h·a₂₂)   Gxy = 1/(h·a₆₆)   νxy = −a₁₂/a₁₁    [a] = [A]⁻¹

These constants are meaningful only for symmetric laminates under in-plane loading. The effective Poisson's ratio of ±θ laminates can be very large (more than 1); a phenomenon that, when plies are combined, leads to interlaminar stresses at edges.

Stiffness design

The book shows that by changing the number and angle of plies, extensional and bending stiffness can be tuned independently: "which plies" for A and "where" for D.

Key pointControl couplings with a symmetric, balanced layup and enough plies. Antisymmetric laminates with few plies cause unexpected behavior and warping in ordinary structures.
NABAK CompositePage 10 of 18
Mechanics of Composite Materials and FRP Composites
Mechanics of Composite Materials

9Laminate strength and hygrothermal effects

Laminate strength analysis procedure

  1. Calculate the stress in each ply under load, including residual thermal and moisture stresses.
  2. Apply a failure criterion (e.g. Tsai-Hill) to each ply and find the first-ply failure load.
  3. Identify the failure mode: if the matrix has failed, that ply's E₂ and G₁₂ are reduced or set to zero; if the fibers have failed, all stiffnesses.
  4. Recalculate laminate stiffness and stresses; continue increasing the load.
  5. Repeat until ultimate failure; a multilinear load-strain curve with "knees" at each ply failure.

The book examines the classic example of a cross-ply laminate in tension: the 90-degree plies crack early (first knee) but the 0-degree plies carry load up to much higher levels. This example shows the difference between "first-ply strength" and "ultimate strength".

Thermal and moisture effects

{σ}ₖ = [Q̄]ₖ({ε⁰} + z{κ} − {α}ₖΔT − {β}ₖΔM)
{N^T} = Σ[Q̄]ₖ{α}ₖΔT(zₖ−zₖ₋₁)    {M^T} = ½Σ[Q̄]ₖ{α}ₖΔT(zₖ²−zₖ₋₁²)
  • Residual cure stresses: cooling from the cure temperature (large negative ΔT) creates transverse tensile stress in the transverse plies, using up part of the Y_t strength.
  • Warping: an unsymmetric laminate bends or twists after cure because of M^T; this is an experimental method for determining residual stresses.
  • Moisture: matrix swelling offsets part of the thermal stress but reduces Tg and matrix properties.

Design for strength

The book introduces laminate "failure envelopes" (Nx-Ny failure plots) and shows how to match the strength envelope to the design load envelope by adjusting the proportions of 0, ±45 and 90 degree plies.

Key pointStrength analysis without residual thermal stresses is incomplete; in many epoxy laminates, residual transverse stress uses up a large part of the transverse strength before any external load is applied.
NABAK CompositePage 11 of 18
Mechanics of Composite Materials and FRP Composites
Mechanics of Composite Materials

10Interlaminar stresses and the free-edge effect

CLT assumes the stresses σz, τxz and τyz are zero. But at the free edge of a laminate (e.g. the edge of a strip in tension), the boundary condition requires τxy, σy and τyz to be zero at the edge, while CLT gives non-zero values in the interior. The transition from interior to edge creates interlaminar stresses in a "boundary layer" about as wide as the laminate thickness.

The classic work of Pipes and Pagano

  • [±45]s laminate in tension: the mismatch in shear coupling of the +45 and −45 plies creates a large interlaminar shear stress τxz near the edge, which peaks at the edge (singular in elastic analysis).
  • Cross-ply laminate: the Poisson's ratio mismatch of the 0 and 90 degree plies creates an interlaminar normal stress σz.

Effect of stacking sequence

The book shows that laminates with the same plies in a different order (e.g. [±15/±45]s versus [±45/±15]s, or [0/90]s versus [90/0]s) have σz of opposite sign. Tensile σz accelerates delamination and compressive σz suppresses it; so the ply sequence, without changing in-plane stiffness, greatly changes fatigue strength and ultimate strength.

Source of interlaminar stressMechanism
Poisson's ratio mismatchNormal stress σz and shear τyz at the edge
Shear coupling mismatchShear τxz at the edge of ±θ laminates
Holes, notches, ply dropsInternal free edges
Joints and thickness changesLoad transfer between plies

Mitigation measures

Choosing a sequence that makes σz compressive, dispersing same-orientation plies rather than stacking them, edge caps, through-thickness stitching, a tough matrix and gradual thickness reduction.

Key pointDelamination starts at edges and holes, where CLT sees nothing. Choose the ply sequence not only for bending stiffness but also for the sign of the interlaminar edge stresses.
NABAK CompositePage 12 of 18
Mechanics of Composite Materials and FRP Composites
Mechanics of Composite Materials

11Bending, buckling and vibration of laminated plates

The book writes the governing equations of laminated plates based on CLT and examines the effect of couplings with exact and approximate solutions for rectangular plates.

D₁₁w,xxxx + 4D₁₆w,xxxy + 2(D₁₂+2D₆₆)w,xxyy + 4D₂₆w,xyyy + D₂₂w,yyyy = p + Nx·w,xx + 2Nxy·w,xy + Ny·w,yy

(For a symmetric laminate; in an unsymmetric laminate the in-plane and bending equations are coupled through B.)

Flexure

  • Specially orthotropic, simply supported: exact double Fourier series (Navier) solution.
  • Symmetric angle-ply: the D₁₆ and D₂₆ terms rule out a closed-form solution; Ritz or Galerkin methods. Ignoring them underestimates deflection.
  • Antisymmetric cross-ply and angle-ply: with suitable boundary conditions, an exact solution exists; B coupling increases deflection, but its effect decreases as the number of plies increases.

Buckling

Nx,cr = π²·[D₁₁m⁴ + 2(D₁₂+2D₆₆)m²R² + D₂₂R⁴] / (a²m²)    R = a/b, n = 1

The number of half-waves m that minimizes the load changes with aspect ratio. The book shows that B coupling in two-ply antisymmetric laminates greatly reduces the buckling load, and with six to eight plies this effect is almost eliminated.

Free vibration

ω²mn = (π⁴/ρh)·[D₁₁(m/a)⁴ + 2(D₁₂+2D₆₆)(m/a)²(n/b)² + D₂₂(n/b)⁴]

The same combination of bending stiffnesses controls deflection, buckling and frequency. The trends with coupling and number of plies are similar to buckling.

The book's approach to approximate solutions

The Ritz energy method with beam functions or polynomials for plates with bend-twist coupling and clamped boundary conditions; its convergence and accuracy are compared with exact solutions.

Key pointThe specially orthotropic assumption (dropping D₁₆, D₂₆ and B) simplifies calculations but makes the results unsafe for angle-ply and antisymmetric laminates with few plies: lower deflection and higher buckling load and frequency than in reality.
NABAK CompositePage 13 of 18
Mechanics of Composite Materials and FRP Composites
Mechanics of Composite Materials

12Fatigue, damage tolerance and fracture mechanics

Fatigue of FRP composites

The fatigue behavior of composites is fundamentally different from metals. In metals one dominant crack grows; in composites, damage is diffuse and multi-mode:

  1. Matrix cracking in transverse and angled plies, up to a "characteristic damage state" (crack saturation at roughly constant spacing).
  2. Crack coupling and delamination where cracks meet adjacent plies and at edges.
  3. Fiber–matrix debonding and growth of local damage.
  4. Fiber breakage and finally rupture.

The result: gradual loss of stiffness, which is a better indicator of damage progression than crack length. Carbon/epoxy laminates dominated by 0-degree fibers have a very flat S-N curve and excellent fatigue life; glass laminates show more loss because of their lower modulus (higher matrix strain) and the sensitivity of glass fibers to moisture. Compression and tension-compression fatigue are usually more severe than tension-tension.

Damage tolerance and impact

  • Low-velocity impacts (dropped tools) can cause extensive internal delamination that is not visible from the surface (barely visible damage).
  • This damage greatly reduces compressive strength; the design criterion is "compression after impact" (CAI) strength.
  • Tough matrices, ±45 plies at the surface, stitching and 3D fibers improve damage tolerance.

Composite fracture mechanics

Linear elastic fracture mechanics works for interlaminar cracks (delamination) with energy release rates G_I and G_II. For cracks perpendicular to the fibers, fracture is more complex because of the damage zone at the crack tip. For the strength of specimens with holes or notches, the semi-empirical Whitney-Nuismer point stress and average stress criteria predict strength with a characteristic length and explain the "hole size effect" (larger hole, lower strength).

Key pointIn composites, damage before failure is extensive and often invisible. Design must control both the "damage initiation threshold" (for durability and moisture ingress) and the "residual strength with damage" (for safety).
NABAK CompositePage 14 of 18
Mechanics of Composite Materials and FRP Composites
Mechanics of Composite Materials

13Transverse shear, environmental effects and joints

Effect of transverse shear

By comparing with Pagano's exact elasticity solutions, the book shows that CLT substantially underestimates deflection for plates with low span-to-thickness ratios and high shear anisotropy (large E₁/G₁₃). Shear deformation theories (Whitney, Reissner-Mindlin) reduce this error by including γxz and γyz. For carbon composites, the shear effect is significant up to span-to-thickness ratios of about 20 to 40.

Environmental effects

  • Moisture: absorption by Fickian diffusion; reduces Tg and matrix-controlled properties.
  • Temperature: loss of matrix stiffness and strength as Tg is approached; the hot-wet combination is the worst case.
  • Thermal cycling: matrix microcracks caused by residual stresses.
  • UV radiation and chemicals: surface degradation of the resin; requires surface veil, coating or a resistant resin.

Joints

TypeFailure modesDesign notes
Bolted / rivetedBearing, net-section tension, shear-out, cleavage, bolt failureEdge distance at least several times the diameter; quasi-isotropic laminate in the joint region; controlled tightening torque
BondedAdhesive shear, peel, delamination of the adherend surface plyStress concentration at the ends of the overlap; stepped or tapered overlaps; surface preparation
Combined—Extra safety, but load is initially carried mainly by the adhesive

The book stresses that joints are often the weakest part of a composite structure, because stress concentrations and interlaminar stresses accumulate there and composites, unlike metals, do not redistribute stress concentrations through local yielding.

Note for FRP profilesIn bolted joints of pultruded profiles, fibers are mainly longitudinal and shear-out and transverse bearing strength are low; sufficient edge and end distances and, where possible, the use of mat or fabric in the walls are essential.
Key pointStart joint design at the start of structural design; the laminate layup in the joint region often needs to differ from the mid-region and lean toward quasi-isotropic.
NABAK CompositePage 15 of 18
Mechanics of Composite Materials and FRP Composites
Mechanics of Composite Materials

14Introduction to composite structural design

The final chapter of Jones's book links mechanics to design. The main message: composite design is the simultaneous design of material and structure and does not succeed through "black aluminum" substitution (copying a metal design in composite).

Design process

  1. Defining requirements: loads (static, fatigue, impact), environment, stiffness and deflection, weight, cost, life and repairability.
  2. Material selection: fiber and matrix suited to the requirements and manufacturing method; lamina properties determined by testing.
  3. Configuration selection: monolithic laminate, sandwich, stiffener-reinforced; overall geometry.
  4. Laminate design: number, angle and sequence of plies.
  5. Joint and detail design.
  6. Analysis: stress, stiffness, stability, vibration, fatigue and damage.
  7. Optimization and iteration.
  8. Testing: a test pyramid from coupons and elements to components and the full structure.

Design analysis philosophy

  • Design criteria: first-ply failure, a strain limit (e.g. about 0.3 to 0.4% for damaged carbon/epoxy) or ultimate strength, depending on the application and the consequences of failure.
  • Statistical allowables: design strengths based on statistics (A-basis and B-basis) and worst-case environmental conditions.
  • Safety factors: larger than for metals because of scatter, damage sensitivity and brittle behavior.

Laminate optimization

The book introduces the problem of finding the layup with the lowest weight or highest buckling load. The variables are discrete (allowed angles and standard ply thickness), so discrete search methods and practical manufacturing constraints are needed. Carpet plots are used to quickly select the percentages of 0, ±45 and 90 plies.

Empirical design rules

  • Symmetric and balanced laminate; at least about 10% of plies in each principal direction.
  • Avoid stacking same-orientation plies; ±45 plies on the outer surface.
  • Gradual ply drops; avoid abrupt stiffness changes.
  • Design for manufacturability and inspection.
Key pointThe biggest mistake in composite design is imitating a metal design. The advantage of composites lies in placing fibers along the load path, integrating parts and choosing a suitable configuration (such as sandwich); the design must be done for composites from the start.
NABAK CompositePage 16 of 18
Mechanics of Composite Materials and FRP Composites
Mechanics of Composite Materials

15Conclusions and frequently asked questions

The book's ten golden points

  1. Macromechanics for structural design and micromechanics for understanding and selecting the material.
  2. Engineering constants have physical restrictions; check data against them.
  3. The invariants U₁ to U₅ show that angle distributes stiffness rather than creating it.
  4. Interactive criteria such as Tsai-Hill and Tsai-Wu agree better with off-axis tests.
  5. Compressive strength is limited by fiber misalignment and transverse strength by matrix strain concentration.
  6. A is independent of sequence, D depends on sequence and B arises from asymmetry.
  7. Residual thermal stresses use up part of the transverse strength.
  8. Interlaminar edge stresses are controlled by the ply sequence and are the origin of delamination.
  9. Fatigue damage is diffuse and stiffness loss is its indicator; CAI is the damage tolerance criterion.
  10. Composite design means designing the material, layup, configuration and joints together.

Applications for FRP product manufacturers

The knowledge in this book lies behind every property table for FRP profiles, panels or tanks: choosing roving and mat percentages (micromechanics and layup), explaining the difference between longitudinal and transverse properties, predicting behavior in hot and wet environments, designing bolted joints and estimating fatigue life.

Frequently asked questions

What is the difference between macromechanics and micromechanics? Macromechanics treats the lamina as a homogeneous anisotropic material with average properties; micromechanics predicts those properties from the interaction of fiber and matrix.

Why do free-edge interlaminar stresses matter? Because they arise at edges from the mismatch in the plies' Poisson's ratios and shear coupling and initiate delamination; the stacking sequence determines their sign.

How does fatigue damage progress in composites? Matrix cracking to saturation, then delamination and fiber–matrix debonding, and finally fiber breakage.

Can a composite's Poisson's ratio exceed 0.5? Yes; in anisotropic materials the restriction is |ν₁₂| < √(E₁/E₂), and in angle-ply laminates it may even exceed 1.

NABAK CompositePage 17 of 18
Mechanics of Composite Materials and FRP Composites
Mechanics of Composite Materials

16Glossary of composite mechanics terms

English termMeaningShort explanation
Composite materialComposite materialMacroscopic combination of two or more materials
Macromechanics / MicromechanicsMacromechanics / micromechanicsApparent behavior / constituent interaction
Lamina / LaminateLamina / laminateSingle ply / ply stack
Specially orthotropicSpecially orthotropicMaterial axes aligned with load
Engineering constantsEngineering constantsE, G and ν
Positive definitenessPositive definitenessCondition for positive energy
Invariants (U₁–U₅)InvariantsAngle-independent terms
Chentsov coefficientsChentsov coefficientsInteraction of shear strains
Tsai–Hill / Hoffman / Tsai–WuTsai-Hill / Hoffman / Tsai-WuInteractive failure criteria
Contiguity factorContiguity factorDegree of fiber contact
Halpin–TsaiHalpin-TsaiSemi-empirical micromechanics equations
Minimum / Critical fiber volumeMinimum / critical volume fractionLimits of fiber effectiveness
MicrobucklingMicrobucklingFiber buckling in compression
CLT / ABDClassical laminate theory / ABD matrixLaminate analysis
Quasi-isotropicQuasi-isotropicDirection-independent A
Free-edge effectFree-edge effectInterlaminar stresses at the edge
Characteristic damage stateCharacteristic damage stateMatrix crack saturation
Compression after impact (CAI)Compression after impact strengthDamage tolerance criterion
Point / Average stress criterionPoint / average stress criterionOpen-hole strength
Bearing / Shear-outBearing / shear-outBolted joint failure
Carpet plotCarpet plotQuick layup design
A-basis / B-basisStatistical allowablesDesign strength

Related keywords: mechanics of composite materials, composite mechanics, composite materials, FRP composites, macromechanics, micromechanics, laminate, Tsai-Wu criterion, interlaminar stress, composite fatigue, damage tolerance, composite joints, composite structural design, FRP profiles, NABAK Composite.

NABAK CompositePage 18 of 18