Pultrusion for Engineers
Pultrusion for Engineers
Pultrusion for Engineers: A Comprehensive Book Summary
From process to structure: resins and fibers, pultrusion machines and dies, process modeling and control, thermoplastic pultrusion, FRP profile properties and standards, structural design of composite profiles, buckling, creep, connections and applications in bridges and buildings
About this book
Whereas the classic pultrusion books focus mainly on "how to produce", this book also answers the end-user engineer's question: "how do I design with FRP profiles?". Its chapters, written by manufacturers, researchers and structural designers, cover the complete chain: pultrusion materials and process, profile properties, structural design principles (especially based on the European EUROCOMP approach), connections and real examples such as all-composite bridges. For FRP profile manufacturers, this book provides a common language with the engineer customer.
How to use this summary
- Orange "Key point" boxes give the most important lesson of each chapter.
- Gold "Note" boxes are supplementary explanations or updates since the book's publication.
- The figures given are typical ranges; for design and product certification, current standards and codes and test data govern.
Pultrusion for Engineers
Table of Contents
- 1Introduction: pultrusion, history and market
- 2Pultrusion resins
- 3Reinforcements and fiber architecture
- 4The pultrusion machine and production line
- 5The pultrusion die and process parameters
- 6Process modeling and control
- 7Thermoplastic pultrusion
- 8Advanced pultrusion variants
- 9Quality control, properties and the EN 13706 standard
- 10Design philosophy and EUROCOMP partial factors
- 11Member design: bending, deflection, shear and buckling
- 12Creep, durability and fire
- 13Bolted connections
- 14Bonded connections and structural systems
- 15Applications in bridges and buildings
- 16Other markets and the future of pultrusion
- 17Conclusions and frequently asked questions
- 18Glossary of pultrusion and FRP design terms
Pultrusion for Engineers
1Introduction: pultrusion, history and market
Pultrusion is a continuous process for producing composite profiles of constant cross-section: continuous fibers (roving, mat and fabric) impregnated with thermoset (or thermoplastic) resin are pulled through a heated die, cured and cut to the desired length after the puller. The product is an FRP profile (fiberglass or GRP profile) with high fiber volume fraction, uniform quality and competitive cost.
A short history
- 1950s: started in the United States to produce solid rods (fishing rods, tool handles).
- 1960s and 1970s: open and hollow profiles by adding mat; electrical and corrosion-resistant markets.
- 1980s and 1990s: large structural profiles, building systems and the first all-composite bridges; development of design guides (such as EUROCOMP in Europe and manufacturers' design manuals in the United States).
Advantages of pultruded profiles
- Light weight: about a quarter of the weight of steel
- Resistance to corrosion and chemicals
- Electrical and thermal insulation; non-magnetic
- Transparency to radio waves
- Fast installation without heavy cranes
- Low maintenance and long life
- Uniform quality in continuous production
- Color throughout the material
Limitations from the engineer's perspective
Low elastic modulus (about 20 to 30 GPa for glass/polyester profiles), anisotropy and transverse weakness, brittle behavior without yielding, sensitive connections, creep under permanent load, fire behavior and the lack of formal design codes at the time the book was published.
Market
The book identifies the main markets as electrical and electronics, corrosion resistance and chemical industries, building and infrastructure, transportation, consumer and leisure goods, and offshore platforms, and links growth in the building market to the availability of design guides and standard profiles.
Pultrusion for Engineers
2Pultrusion resins
A pultrusion resin must have conflicting properties: low viscosity and long working life in the bath or injection chamber, and very fast cure (in under a minute) in the heated die. It also determines the final properties (mechanical, chemical, fire).
| Resin | Process characteristic | Properties and applications |
|---|---|---|
| Isophthalic polyester | Fast cure, cheap, filler tolerance | The most widely used; structural profiles and general grating |
| Orthophthalic polyester | The cheapest | Less demanding applications; limited chemical resistance |
| Vinyl ester | Slightly slower; lower shrinkage | High corrosion resistance and toughness; chemical environments |
| Epoxy | Slow cure; low line speed; sticks to the die | Best mechanical and electrical properties; carbon/epoxy, insulators |
| Phenolic | Condensation cure releasing water; difficult process | Excellent fire, smoke and toxicity behavior; offshore platforms, tunnels, metros |
| Modified acrylic | Low viscosity; high speed | Good fire behavior with ATH filler; weathering resistance |
| Polyurethane | Very fast; requires closed injection | High toughness and strength (a growing trend) |
Formulation components
- Initiators: a combination of low- and high-temperature peroxides for rapid gelation and full cure.
- Internal release: prevents sticking and reduces pull force.
- Fillers: calcium carbonate and kaolin for cost and lower shrinkage; ATH for fire retardancy and smoke reduction.
- Low-profile additive, pigment and UV absorber.
Selection criteria
Service environment (chemical, UV, temperature), fire requirements, mechanical properties, production speed and cost. The book stresses that resin selection is an "economic balance": vinyl ester or phenolic cost more but, in the right application, greatly increase life and safety.
Pultrusion for Engineers
3Reinforcements and fiber architecture
Types of reinforcement
| Reinforcement | Role in the profile |
|---|---|
| Unidirectional continuous roving | Longitudinal strength and stiffness; transmits pull force in the line |
| Continuous filament mat (CFM) | Transverse strength and stiffness; resistance to splitting; holds the rovings together |
| Chopped strand mat (CSM) | Similar to CFM; its binder must be stable in styrene |
| Woven and multiaxial stitched fabrics (±45, 0/90) | Higher shear and transverse properties; bearing resistance at connections |
| Surface veil (polyester or C-glass) | Resin-rich layer; UV and chemical resistance; better appearance |
| Carbon and aramid fibers | High stiffness (carbon) or impact resistance (aramid); special applications |
Ply architecture in the profile
A typical pultruded profile wall has a symmetric layered structure: surface veil, mat or stitched fabric, a roving core, then mat and veil again. The ratio of roving to mat determines the balance of longitudinal and transverse properties:
- More roving: higher longitudinal modulus and strength; transverse weakness and splitting.
- More mat or stitched fabric: better transverse, shear and bearing properties; lower total volume fraction.
Volume fraction and properties
Fiber weight fraction in structural profiles is usually about 50 to 70 percent. In unidirectional rods up to about 80 percent by weight is possible. Longitudinal properties are predicted roughly by the rule of mixtures and transverse properties by the contribution of the mat and stitched layers.
Sizing and compatibility
The fiber sizing must be compatible with the resin (silanes specific to polyester, vinyl ester or epoxy); incompatibility slows wet-out and reduces shear properties and durability in water.
Pultrusion for Engineers
4The pultrusion machine and production line
Line components
- Creel: holds roving packages and mat rolls with uniform tension.
- Guides and separator plates: set the fiber path.
- Impregnation: open (dip) bath or an injection chamber attached to the die.
- Preformers: gradually guide the wet fibers into the section shape and remove excess resin.
- Heated die: shaping and cure; multi-zone heating.
- Cooling zone: sufficient distance before the puller.
- Puller: caterpillar (continuous belt) or reciprocating clamp (hydraulic or electric).
- Flying cut-off saw: cuts while moving, with dust extraction.
Open bath versus injection
| Feature | Open bath | In-die injection |
|---|---|---|
| Simplicity and cost | Simple and cheap | More complex; requires chamber design |
| Styrene emissions | High | Very low |
| Fast resins (PU, special phenolics) | Impossible or difficult | Possible |
| Color and resin changes | High waste | Low waste |
| Impregnating thick fabrics | Good | Requires precise pressure design |
Machine specifications
- Pull capacity: from a few tonnes for rods to tens of tonnes for wide, thick profiles.
- Section envelope: maximum producible width and height; large profiles over a meter wide on special machines.
- Speed: usually a fraction of a meter to a few meters per minute; thick profiles slower.
- Multi-cavity production: several small profiles at once to increase productivity.
Pultrusion for Engineers
5The pultrusion die and process parameters
Die design
- Material: tool steel with hard chrome plating for wear resistance and a smooth surface.
- Length: usually about 60 to 120 cm; a longer die allows higher speed but more friction and cost.
- Entrance: tapered or flared for gradual compaction and removal of excess resin.
- Cavity dimensions: allowing for resin shrinkage and steel thermal expansion.
- Multi-piece construction: for machining, cleaning and repair; mandrel for hollow sections.
- Heating: platen or cartridge heaters in several independent zones; entrance cooling.
Material behavior in the die
The material passes through three zones in turn: liquid (heating and compaction), gel (start of cure and maximum adhesion to the wall) and solid (cure, shrinkage and release from the wall). The peak cure exotherm raises the profile center temperature above the wall. The aim is to place gelation and peak exotherm at the right point along the die.
Key process parameters
| Parameter | Effect |
|---|---|
| Pulling speed | Residence time in the die; higher speed, less cure at the exit |
| Die zone temperatures | Gel and peak location; excessive temperature, cracking and sticking |
| Resin formulation and initiators | Reactivity and process window |
| Fiber fill | Pull force, surface quality, properties |
| Preheating (RF or microwave) | Higher speed in thick sections |
Common defects
Surface and internal cracks, surface sloughing (sticking to the die), incomplete cure, blisters, dry fibers, fiber prominence, twisting and bowing, and dimensional deviation. Most defects are rooted in a shifted gel point, insufficient release or improper fiber fill.
Pultrusion for Engineers
6Process modeling and control
The book devotes a chapter to modeling the pultrusion process so that line setup moves from trial and error to scientific prediction.
Thermo-chemical model
With cure kinetics data from DSC testing and thermal properties, the distribution of temperature and degree of cure along the die and across the section is predicted. Outputs: gel location, peak exotherm, exit degree of cure and maximum allowable speed.
Flow and impregnation model
Resin flow in the fiber bed with Darcy's law; for designing the tapered die entrance and injection chambers and predicting pressure, fiber wet-out and void risk.
Pull force model
The sum of fiber compaction resistance at the entrance, viscous drag of the liquid resin, adhesion in the gel zone and friction in the solid zone. The most sensitive part is the gel zone.
Process control
- Monitoring temperature (die thermocouples and a trailing thermocouple), speed and pull force.
- Dielectric or ultrasonic sensors to detect cure in the die.
- Feedback control of die zone temperatures based on speed and pull force.
- Statistical process control (SPC) for dimensions and properties.
Optimization
Using the models, die zone temperatures and speed are chosen so that exit degree of cure is sufficient, maximum temperature stays below the degradation limit and speed is maximized; for thick sections, preheating and multi-stage initiators are considered.
Pultrusion for Engineers
7Thermoplastic pultrusion
In thermoplastic pultrusion, instead of chemically curing, the matrix melts, impregnates the fibers and then solidifies on cooling. The main challenge is the very high viscosity of thermoplastic melts (hundreds to thousands of times that of thermoset resins), which makes impregnation difficult.
Impregnation methods
| Method | Description |
|---|---|
| Pre-impregnated tapes | Fully impregnated tapes (such as carbon/PEEK or glass/PP) are only melted and consolidated; the best quality, the most expensive |
| Commingled yarns | Fiber filaments and polymer filaments side by side; short flow distance |
| Powder impregnation | Polymer powder is deposited on the fibers and melted |
| Melt impregnation | Fibers pass through melt in an injection chamber with spreading pins |
| In-situ polymerization | A low-viscosity monomer (such as caprolactam for PA6) that polymerizes in the die |
Stages of a thermoplastic line
- Preheating fibers and polymer (infrared or hot air).
- Hot die for complete melting, impregnation and consolidation under pressure.
- Cold die for solidification under pressure and to fix dimensions and surface quality.
- Pulling and cutting.
Advantages and limitations
- Advantages: no styrene emissions; high toughness and impact resistance; secondary forming (bending profiles with heat), welding and recycling are possible.
- Limitations: usually lower speed; cost of intermediate materials; high process temperature; creep of matrices such as PP; crystallization control.
Pultrusion for Engineers
8Advanced pultrusion variants
| Process | Principles | Products |
|---|---|---|
| Pull-winding | Combining longitudinal pulling with hoop or helical winding of fibers on a mandrel before the die | Pressure pipes, shafts and poles with high hoop strength |
| Pull-braiding | In-line circular braiding of ±θ fibers over a longitudinal core | Tubes and profiles with torsional and impact resistance |
| Pulforming | Shaping pulled material in moving or rotating molds | Parts with variable section, leaf springs |
| Curved pultrusion | Curved die and puller | Arched parts with constant radius |
| RF and microwave preheating | Volumetric heating of material before the die | Higher speed for thick sections |
| In-die resin injection | Closed, pressurized impregnation | Lower emissions; fast resins |
| Pultrusion with foam cores or inserts | Passing a light core or metal parts through with the fibers | Continuous sandwich panels, insulated window profiles |
Wide profiles and panels
Wide multi-cell panels (for floors, bridge decks, walls and roofs) are produced with large dies and powerful pullers. Building systems based on interlocking panels make rapid construction of complete structures possible (chapter 14).
Carbon pultrusion
Carbon rods and strips for strengthening concrete structures, wind turbine blade spar caps and lightweight applications; require epoxy or vinyl ester resin and precise control of fiber tension and cure.
FRP rebar
Glass, basalt or carbon rebar with ribbed, sand-coated or wrapped surfaces for bond to concrete; a substitute for steel in corrosive environments (bridges, docks, tunnels).
Pultrusion for Engineers
9Quality control, properties and the EN 13706 standard
Typical properties of glass/polyester profiles
| Property | Longitudinal | Transverse |
|---|---|---|
| Tensile modulus (GPa) | ~20–28 | ~6–10 |
| Tensile strength (MPa) | ~200–400 | ~50–80 |
| Compressive strength (MPa) | ~200–400 | ~70–140 |
| Flexural strength (MPa) | ~200–400 | ~70–140 |
| In-plane shear modulus (GPa) | ~3–4 | |
| Interlaminar shear strength (MPa) | ~25–35 | |
| Density (g/cm³) | ~1.7–2.0 | |
The EN 13706 standard
The European specification standard for pultruded profiles, which was being drafted when the book was published and was issued later. It has three parts: designation, test methods and requirements. It defines two quality grades:
| Grade | Minimum longitudinal tensile modulus | Application |
|---|---|---|
| E23 | ~23 GPa | Structural applications |
| E17 | ~17 GPa | General and non-structural applications |
Besides modulus, minimum longitudinal and transverse tensile and flexural strengths, pin-bearing strength, interlaminar shear, and dimensional and visual tolerances (based on methods similar to ASTM D4385 for visual defects) are specified. Check the exact values in the current text of the standard.
Quality control tests
- Barcol hardness for degree of cure; fiber content by burn-off; density.
- Tensile, flexural, interlaminar shear (short beam) and pin-bearing tests on specimens cut from the profile.
- Dimensional (thickness, bow, twist, flatness) and visual inspection.
- Full-section profile testing (beam bending) to determine effective bending and shear stiffness.
Pultrusion for Engineers
10Design philosophy and EUROCOMP partial factors
The book describes the structural design of FRP profiles mainly on the basis of the EUROCOMP design code and handbook (published in Europe in the 1990s), which applies the limit state principles of European codes to FRP composites.
Limit states
- Ultimate limit state (ULS): material failure, buckling, connection failure; under factored loads.
- Serviceability limit state (SLS): deflection, vibration, cracking and appearance; usually governs in FRP.
Material partial factors
| Factor | Source of uncertainty | Description |
|---|---|---|
| γ_m1 | How properties are determined | Lower for properties tested on the profile; higher for properties calculated from theory |
| γ_m2 | Manufacturing and cure process | Pultrusion with good quality control and full post-cure has a lower factor than hand lay-up |
| γ_m3 | Environment and load duration | Long-term load and high temperature, a larger factor; short-term load, a smaller factor |
The product of these factors for long-term loads can be noticeably larger than steel's factors; this reflects FRP's greater scatter, environmental sensitivity and creep.
Characteristic values
Characteristic property values are obtained from testing with statistical analysis (e.g. the fifth percentile at a specified confidence); the producer should provide them for each profile and direction.
Pultrusion for Engineers
11Member design: bending, deflection, shear and buckling
Deflection: usually governs
With a longitudinal modulus about one-tenth of steel and a low shear modulus, FRP beam deflection usually governs before strength. Deflection must be calculated with Timoshenko theory, including the shear contribution:
A_w is the web area and k the shear coefficient. For short spans, the shear contribution can exceed ten percent. Typical deflection limits are about L/250 to L/400 depending on the application. The effective E and G of the full profile are best obtained from full-section bending tests at several spans.
Flexural and shear strength
Bending stresses in the flanges are checked against the characteristic longitudinal strength, and shear stress in the web against the in-plane shear strength. Stress concentration at the flange-web junction (corners) and the transverse weakness of the walls must be checked.
Buckling
| Mode | Importance in FRP profiles |
|---|---|
| Local buckling of the compression flange | Orthotropic plate flange with one free edge; often governs flexural capacity |
| Local buckling of the web | Under shear or bending compression in deep beams |
| Lateral-torsional buckling | Open beams without lateral restraint; important because of low torsional stiffness |
| Global column buckling (Euler) | With a low modulus, the critical load is low; the shear effect lowers it further |
| Local-global interaction | In columns of intermediate slenderness |
| Web crippling | At supports and under concentrated loads; requires stiffeners |
The local buckling capacity of flanges is calculated with orthotropic plate theory (taking into account the rotational restraint of the flange-web junction). The book gives semi-empirical relations and test results for I and channel profiles.
Pultrusion for Engineers
12Creep, durability and fire
Creep
Under permanent load, FRP profiles creep because of the viscoelasticity of the resin; creep is limited in the longitudinal (fiber-controlled) direction but greater in shear and transversely. The common empirical model is Findley's power law:
ε₀ is the instantaneous strain and m and n are material constants (n usually about 0.2 to 0.3). With this model, the effective long-term (e.g. 50-year) modulus is obtained for calculating long-term deflection. Higher temperature and humidity accelerate creep. Long-term working stress must be limited to a fraction of the short-term strength to prevent creep rupture.
Durability
- Moisture and water: reduce matrix-controlled properties; surface veil, a suitable resin and full cure are important.
- UV and weathering: yellowing and fiber blooming; surface veil, UV absorber or paint.
- Chemicals: vinyl ester for corrosive environments; ECR glass in acidic environments.
- Alkali (concrete): for glass FRP rebar, alkali-resistant resin and fibers are needed.
- Temperature: design with sufficient margin below the resin's Tg.
Fire behavior
Polymer resins are combustible and profile properties drop rapidly at temperatures near Tg (usually about 80 to 120 °C for polyester and vinyl ester). Remedies: phenolic or fire-retardant acrylic resin, ATH filler, intumescent coatings and insulation. Reaction-to-fire classification (such as Euroclass or ASTM E84) and the fire resistance of load-bearing members must be checked separately.
Pultrusion for Engineers
13Bolted connections
Connections are the most sensitive part of FRP profile structures. The book examines bolted connections based on extensive laboratory research (especially at UK universities).
Failure modes of bolted connections
| Mode | Cause | Design control |
|---|---|---|
| Bearing | Bolt pressure on the hole wall | The preferred mode (progressive and relatively ductile) |
| Net-section tension | Little remaining width | Sufficient edge distance and width |
| Shear-out | Small end distance; fibers mainly longitudinal | Large end distance; transverse plies |
| Cleavage | Combination of transverse tension and shear | Sufficient mat and stitched plies |
| Bolt failure or pull-through | Weak bolt or low thickness | Stainless steel bolt; large washer |
Influencing factors
- Distances: ratio of end distance to diameter (e/d) and width to diameter (w/d); typical recommended values are several times the diameter (for example, an end distance of about 3 to 5 times the diameter).
- Load direction relative to the fibers: load perpendicular to the fibers gives lower bearing and shear-out capacity.
- Tightening torque and washers: lateral clamping increases bearing capacity; but relaxation occurs over time.
- Hole clearance: low clearance improves load sharing between bolts.
- Multiple bolt rows: unequal load sharing between rows; the first row takes the most load.
Construction details
Drill with diamond or carbide tools and a backing plate to prevent delamination; seal cut edges with resin; use FRP or stainless steel angles and connection plates; avoid galvanic corrosion (where carbon profiles contact metal).
Pultrusion for Engineers
14Bonded connections and structural systems
Adhesive joints
- Advantages: more uniform load distribution, no holes weakening the section, sealing, better appearance.
- Adhesives: structural epoxies and acrylics, and polyurethanes.
- Stress concentration: shear and peel stress at the ends of the overlap; failure often occurs in the profile's surface layer (veil or mat delamination) rather than in the adhesive.
- Surface preparation: sanding and removing surface release agent from the profile are vital; a peel ply is useful in producing profiles intended for bonded connections.
- Durability: effects of moisture, temperature and creep on the adhesive; long-term data are needed.
Hybrid connections
Combining adhesive and bolts: bolts for safety (a second load path) and to hold parts while the adhesive cures; in the intact state, load is carried mainly by the adhesive.
Prefabricated structural systems
The book introduces systems in which profiles interlock with special connectors. The leading example is the Advanced Composite Construction System (ACCS) in the UK: pultruded multi-cell panels with connector "keys" and adhesive, used modularly to build bridge decks, walls and lightweight buildings.
Connection design principles
| Principle | Description |
|---|---|
| Load transfer along the fibers | As far as possible, transfer load through shear or longitudinal tension |
| Avoid transverse tension and peel | Details that pull the wall through its thickness are weak |
| Local reinforcement | Connection plates, thick angles, extra plies |
| Construction and inspection | A connection that cannot be executed and checked on site is not reliable |
Pultrusion for Engineers
15Applications in bridges and buildings
Composite bridges
The book examines pioneering bridges built with pultruded profiles:
- Aberfeldy footbridge (Scotland, 1992): the first all-composite cable-stayed bridge, with a main span of over 60 meters; deck and towers from ACCS panels and aramid cables; rapid installation with light equipment.
- Bonds Mill lift bridge (UK): a composite road lift bridge whose light weight allowed a simpler mechanical system.
- Numerous footbridges in Europe and America with standard profiles; and road bridge decks from wide pultruded panels to replace deteriorated decks.
Lessons: fast, low-cost installation, resistance to corrosion and de-icing salts, and the need for careful design for vibration (light bridges are sensitive to pedestrian-induced vibration) and connections.
Building and industry
| Application | Key advantage |
|---|---|
| Cooling tower structures | Resistance to moisture and chemicals |
| Grating, stairs, handrails and access platforms | Corrosion resistance, light weight, anti-slip, easy installation |
| Chemical industrial structures and treatment plants | Long life without painting |
| Radio-transparent buildings | No interference with antennas and sensitive equipment |
| Window and door profiles | Excellent thermal insulation and dimensional stability |
| Rebar and concrete reinforcement | Corrosion resistance in marine and saline environments |
| Prefabricated and lightweight buildings | Easy transport and installation in remote areas |
Pultrusion for Engineers
16Other markets and the future of pultrusion
Main markets
- Electrical and electronics: ladder rails, cable trays, insulators and cable cores, transformer and switchboard profiles; the advantage of insulation.
- Transportation: body components for refrigerated trucks, trains and buses, springs, impact beams; the advantage of light weight and thermal insulation.
- Offshore platforms: phenolic grating, handrails and stairs for low weight, corrosion resistance and fire behavior.
- Consumer and sporting goods: tool handles, fishing rods, tent poles and flagpoles.
- Agriculture: trellis stakes, fence posts, greenhouse structures.
- Energy: carbon profiles for wind turbine blades and components of solar structures (a trend since the book).
Drivers of market growth
- Standards and design codes that earn the trust of designers and clients.
- Cost reduction through higher production speed, automation and more efficient resins.
- Training engineers to design specifically for FRP (not to copy steel).
- Standard structural and connection systems.
- Long-term durability data and performance records from completed projects.
- Environmental considerations: reducing styrene emissions, recycling and life-cycle assessment.
Technology trends
Injection pultrusion with polyurethane and acrylic resins, larger and more complex profiles, carbon pultrusion, thermoplastics, automatic process control and simulation, and combining pultrusion with other processes (braiding, winding, forming).
Pultrusion for Engineers
17Conclusions and frequently asked questions
The book's ten golden points
- An FRP profile is not lightweight steel; it has low stiffness and high strength and needs its own design approach.
- Choose the resin by environment and fire requirements and the fibers by load.
- The balance of roving and mat or stitched fabric determines longitudinal and transverse properties and connection behavior.
- Monitor pull force, temperature and speed continuously; modeling defines the process window.
- Thermoplastic pultrusion suits toughness, secondary forming and recycling.
- The EN 13706 standard (grades E23 and E17) is the common language of producer and designer.
- Design uses limit states and partial factors that depend on data source, process and load duration.
- Deflection (with shear) and local buckling usually govern; an FRP section is deeper than the equivalent steel section.
- Account for creep and long-term durability with long-term properties.
- Connections are the sensitive point; make bearing the governing mode and use tested connection systems.
Frequently asked questions
What is EN 13706? The European specification standard for pultruded profiles, with two grades, E23 and E17, based on minimum tensile modulus and minimum strengths, together with test methods and tolerances.
Why is FRP beam design usually governed by deflection? Because the elastic modulus is about one-tenth of steel's and the shear modulus is low; deflection and buckling govern before strength.
How do bolted connections in FRP profiles fail? By bearing, net-section tension, shear-out or cleavage; sufficient end and edge distances and enough transverse plies make bearing the governing mode.
How does this book differ from books on pultrusion production? Besides the process, it addresses the end-user engineer's needs: standardized properties, structural design, connections and real applications.
Pultrusion for Engineers
18Glossary of pultrusion and FRP design terms
| English term | Meaning | Short explanation |
|---|---|---|
| Pultrusion / Pultruded profile | Pultrusion / pultruded profile | Continuous production of FRP profiles |
| Roving / CFM / Stitched fabric / Veil | Roving / continuous mat / stitched fabric / veil | Reinforcements |
| Resin bath / Injection die | Resin bath / injection die | Impregnation methods |
| Preformer / Die / Puller | Preformer / die / puller | Line components |
| Pulling force | Pull force | Indicator of process health |
| Thermoplastic pultrusion | Thermoplastic pultrusion | Melting and solidification instead of cure |
| Commingled yarn | Commingled yarn | Fibers and polymer side by side |
| Pull-winding / Pull-braiding / Pulforming | Pull-winding / pull-braiding / pulforming | Advanced variants |
| EN 13706 (E23, E17) | European profile standard | Quality grades |
| EUROCOMP | European design code and handbook | Limit state design of FRP |
| Partial safety factor (γm) | Material partial factor | γm1 × γm2 × γm3 |
| ULS / SLS | Ultimate / serviceability limit state | Design philosophy |
| Shear deformation | Shear deformation | Shear contribution to deflection |
| Local / Lateral-torsional buckling | Local / lateral-torsional buckling | Instability modes |
| Web crippling | Web crippling | Under concentrated load |
| Findley power law | Findley power law | Creep model |
| Bearing / Net-tension / Shear-out / Cleavage | Bearing / net tension / shear-out / cleavage | Bolted joint failure |
| Pin-bearing strength | Pin-bearing strength | Connection test |
| Peel stress | Peel stress | Bonded connection |
| ACCS | Advanced Composite Construction System | Interlocking panels |
| FRP rebar | FRP rebar | Concrete reinforcement |