Handbook of Pultrusion Technology
Handbook of Pultrusion Technology
A Comprehensive, Professional Summary of the Handbook of Pultrusion Technology
A summary for a complete introduction to the pultrusion process for FRP composites: from raw materials and die design to quality control, troubleshooting and production economics
Who is this summary for?
For the process engineer, senior line operator, quality control specialist, product designer and production manager who wants the book's logic and practical points in hand without reading the full text. The chapter order follows the path a profile takes through the plant: material selection, fiber preparation, impregnation, forming and curing in the die, pulling and cutting, and finally testing and cost analysis.
How to use it
- Orange "Key point" boxes are the things that have the greatest effect on quality and cost in practice.
- Gold "Note" boxes are supplementary explanations or updates since the book's publication and are kept separate from the main text.
- The figures in the tables are "typical industrial ranges", not definitive specifications; for each resin and fiber system they must be confirmed with supplier data and line trials.
- Technical terms are given alongside their definitions to make it easy to refer to the original book and catalogs.
Handbook of Pultrusion Technology
Table of Contents
- 1Introduction, definition and history of pultrusion
- 2Markets and applications of pultruded products
- 3Resins: polyester, vinyl ester, epoxy and other systems
- 4Cure chemistry, initiators and additives
- 5Reinforcements: roving, mat, surface veil and advanced fibers
- 6Overview of the pultrusion line
- 7Fiber impregnation and preforming
- 8Die design and manufacture
- 9Thermal profile and cure behavior in the die
- 10Pulling system, saw and machinery
- 11Formulation and fiber layup calculations
- 12Product design and mechanical properties
- 13Quality control and testing
- 14Process troubleshooting
- 15Production economics, safety and environment
- 16Advanced processes and outlook
- 17Conclusions and line start-up checklist
- 18Glossary
Handbook of Pultrusion Technology
1Introduction, definition and history of pultrusion
Definition
The word Pultrusion combines Pull and Extrusion. In extrusion, material is "pushed" through a die; in pultrusion, continuous fibers impregnated with thermoset resin are "pulled" through a heated die, where they are shaped and cured, emerging as a profile of constant cross-section and unlimited length. The final product is a fiber-reinforced polymer composite (FRP).
A brief history
- 1950s: the first work was done in the United States to produce solid glass/polyester rods (mainly for fishing rods and tool handles). W. Brandt Goldsworthy is known as the "father of pultrusion".
- 1960s: adding continuous strand mat to roving made it possible to produce open and hollow profiles (channels, angles, tubes) with acceptable transverse strength.
- 1970s and early 1980s: rapid market growth in the electrical and corrosion-resistant industries; the arrival of vinyl ester resin, better internal release agents and continuous pullers increased speed and quality. Meyer's book was published at this point as one of the first comprehensive references for the industry.
Advantages of pultrusion over other composite processes
- Continuous, automated process with little labor
- High fiber content (up to about 70–80% by weight) and therefore high strength
- Uniform quality and dimensions along the length
- Low material waste
- High strength-to-weight ratio, corrosion resistance, electrical and thermal insulation
- No painting needed (pigment in the resin)
- Non-magnetic and transparent to radio waves
- Low unit cost at high volumes
Limitations
The cross-section must be constant along the length; fibers lie mainly in the longitudinal direction, so transverse properties are weaker; die and setup costs are not justified for low volumes; and line speed drops for thick sections because of heat transfer limits.
Handbook of Pultrusion Technology
2Markets and applications of pultruded products
The book classifies the market by FRP's "key advantage"; that is, customers usually come to pultrusion for one specific property (insulation, corrosion resistance or light weight) and compare price with steel, aluminum or wood.
| Market segment | Key advantage | Example products |
|---|---|---|
| Electrical and electronics | Electrical insulation, non-magnetic | Electricians' ladder rails, insulator and cable cores, cable trays, transformer and switchboard profiles, fire hose |
| Corrosion and chemical resistance | Resistance to acids, alkalis and salt | Grating, stairs and handrails, cooling tower structures, water and wastewater treatment facilities |
| Building and construction | Light weight, durability, thermal insulation | I- and H-beams, window and door frames, FRP rebar, bridge and pedestrian decks |
| Transportation | Strength-to-weight ratio | Truck and refrigerated body components, springs and rods, train interior parts |
| Consumer and sporting goods | Flexibility, good fatigue | Fishing rods, tool handles, tent poles, golf shafts, flag poles and stakes |
| Agriculture | Resistance to fertilizer and moisture | Vineyard trellis stakes, fence posts, greenhouse profiles |
| Aerospace and defense | Very high specific strength | Carbon/epoxy profiles, antenna and radome components |
Market entry logic
- Material substitution: the greatest success is where steel rusts, aluminum conducts electricity or wood rots; life-cycle cost (not just initial price) is the basis for comparison.
- Design for pultrusion: many early failures came from directly copying a steel section. The stiffness (modulus) of glass FRP is about one-tenth that of steel, so the section must be redesigned to control deflection.
- Standard versus custom profiles: standard profiles (angle, channel, tube, I) have high volume and competitive pricing; custom profiles have higher margins, but the die cost must be covered by the customer or by volume.
Handbook of Pultrusion Technology
3Resins
The matrix resin holds the fibers together, transfers load between them and determines chemical, thermal and fire resistance and surface quality. In pultrusion, besides its final properties, the resin must meet three process conditions: suitable viscosity for rapid fiber wet-out, long working life (pot life) in the bath, and very fast cure at die temperature.
| Resin | Process characteristics | Properties and applications |
|---|---|---|
| Orthophthalic unsaturated polyester (Orthophthalic) | Cheap, fast cure, high shrinkage (about 7–8% by volume) | General, low-cost products; limited chemical resistance |
| Isophthalic polyester (Isophthalic) | The most widely used pultrusion resin; good filler tolerance | Better strength and chemical and water resistance than ortho; structural profiles and grating |
| Vinyl ester (Vinyl Ester) | Slightly slower and more expensive, lower shrinkage | Excellent corrosion resistance, better toughness and fatigue; severe chemical environments |
| Epoxy (Epoxy) | Slow cure, higher die temperature, strong adhesion to the die, low line speed | Best mechanical and electrical properties and fiber adhesion; carbon/epoxy, insulators and aerospace parts |
| Phenolic (Phenolic) | Condensation cure releasing water; more difficult process | Excellent fire resistance, low smoke and toxicity; tunnels, mines, offshore platforms |
| Methacrylate / acrylic | Low viscosity, fast cure | Good weathering resistance and colorability |
Key points for resin selection
- Styrene monomer in polyester and vinyl ester is both a solvent (viscosity reducer) and the crosslinking agent. Increasing it lowers viscosity but increases shrinkage and vapor emissions.
- Cure shrinkage makes the part separate from the die wall; some shrinkage helps reduce friction, but high shrinkage causes cracking, fiber print-through and warping. Epoxy has low shrinkage, which is why it sticks to the die and needs a stronger release agent.
- Viscosity for bath impregnation is usually kept in the range of a few hundred to about 2000–3000 centipoise; fillers raise viscosity rapidly.
- Reactivity (gel time and peak exotherm temperature) must be chosen to suit die length and the desired speed; get this data from the supplier through the SPI test or DSC.
Handbook of Pultrusion Technology
4Cure chemistry, initiators and additives
Cure mechanism of polyester and vinyl ester
Cure is by free-radical polymerization. An organic peroxide decomposes with heat and produces radicals; the radicals link the double bonds of the polyester and styrene. After an induction time (consumption of inhibitors), the material gels, then the temperature rises through the exothermic reaction to the peak exotherm and the material hardens.
Initiators (catalysts)
In pultrusion, unlike hand lay-up, cobalt accelerators are usually not used and cure is purely thermal. The book emphasizes using a two- or three-initiator system:
- Low-temperature initiator (such as peroxydicarbonates): starts the reaction early, at the start of the die, for rapid gelation.
- Medium-temperature initiator (such as benzoyl peroxide): a bridge between the two stages.
- High-temperature initiator (such as tert-butyl perbenzoate): completes the cure at the end of the die and reduces residual monomer.
Total initiator is usually about 0.5 to 2 parts per hundred parts of resin (phr). Too much initiator shortens bath life and increases the risk of thermal cracking; too little leads to incomplete cure.
Additives
| Additive | Role | Typical amount |
|---|---|---|
| Internal mold release (Internal mold release) | Migrates to the surface and reduces friction and adhesion to the die; e.g. zinc stearate or phosphate esters | ~0.5–2 phr |
| Fillers (calcium carbonate, kaolin, talc) | Lower cost, lower shrinkage and exotherm, better surface, crack prevention | About 10–40 phr and sometimes more |
| Alumina trihydrate (ATH) | Flame retardant and smoke suppressant by releasing water | Up to about 50 phr or more |
| Low-profile additive (LPA) | Compensates shrinkage, smoother surface, less fiber print-through | A few to 15 phr |
| Pigment (color paste) | Uniform color through the whole volume | ~1–5 phr |
| UV absorber | Reduces yellowing and "fiber blooming" outdoors | Less than 1 phr |
| Wetting agents and viscosity reducers | Improve fiber wet-out in filled formulations | As recommended by the manufacturer |
Handbook of Pultrusion Technology
5Reinforcements
The reinforcement is the composite's main load-carrier and, in pultrusion, it is what gets pulled; so besides strength, it must have enough tensile strength in the "dry and partly wet" state not to break along the path.
Forms of reinforcement
- Continuous roving (Roving): parallel bundles of E-glass filaments. It provides longitudinal strength and stiffness, and the pull force is transmitted through it. Its linear weight is expressed in "tex" (grams per kilometer) or "yield" (yards per pound); e.g. 4400 tex ≈ 113 yd/lb and 2200 tex ≈ 225 yd/lb.
- Continuous strand mat (Continuous Strand Mat, CSM): random swirled continuous strands with a binder. It provides transverse strength and resistance to splitting. The mat must have a binder that is insoluble or poorly soluble in styrene so it does not fall apart in the bath.
- Fabric and woven roving (Woven Roving) and multiaxial stitched fabrics: higher transverse and shear properties; more expensive and harder to preform.
- Surface veil (Surfacing Veil): a thin layer of C-glass or nonwoven polyester at the outer surface; it creates a resin-rich layer, reduces fiber print-through and water absorption, and increases UV and corrosion resistance.
Fiber material
| Fibers | Density (g/cm³) | Tensile modulus (GPa) | Considerations |
|---|---|---|---|
| E-glass | ~2.54–2.60 | ~72–76 | The most economical and common; electrical insulator |
| S-glass | ~2.49 | ~85–89 | Higher strength; more expensive |
| Carbon | ~1.75–1.80 | About 230 and higher | Very high stiffness; electrically conductive; high price |
| Aramid | ~1.44 | ~70–125 | Light and tough; weaker adhesion and difficult to cut |
Sizing and compatibility
The surface of glass fibers is coated with a sizing containing a silane coupling agent. The sizing must be compatible with the resin chemistry (polyester, vinyl ester or epoxy); an unsuitable sizing causes slow wet-out, white fibers and loss of interlaminar shear strength.
Handbook of Pultrusion Technology
6Overview of the pultrusion line
A pultrusion line consists of stations in series, all working at one constant speed. The following order is the path the fibers take:
| Station | Function | Control point |
|---|---|---|
| Roving creel and mat holder (Creel) | Continuous feeding of fibers and mat rolls | Uniform tension; preventing twisting and contact with sharp edges |
| Guides (Guides / Card plates) | Arranging and separating strands | Polished holes (ceramic, PTFE or chrome steel) |
| Resin bath (Resin bath) | Complete fiber impregnation | Temperature, viscosity, resin level and residence time |
| Preformer (Preformer) | Removing excess resin and bringing the shape close to the final section | Alignment with the die axis; correct placement of mat and veil |
| Heated die (Heated die) | Compaction, shaping and cure | Multi-zone temperature profile |
| Puller (Puller) | Applying pull force at constant speed | Appropriate clamp pressure; recording pull force |
| Cut-off saw (Cut-off saw) | Cutting to the desired length | Moves in sync with the line; diamond or abrasive blade; dust extraction |
Handbook of Pultrusion Technology
7Fiber impregnation and preforming
Impregnation methods
- Open dip bath (Dip bath): the most common method at the time of the book. Fibers pass under bars through the resin. It is simple and cheap but has a large open surface for styrene evaporation.
- Straight-through bath (Straight-through bath): fibers pass through the resin without bending; better for mat and fabric, because bending over bars shifts and wrinkles them.
- In-die resin injection (Resin injection): resin is pumped directly into the start of the die. Lower emissions and the possibility of using fast resins; it became more widespread later.
Factors affecting wet-out
Impregnation quality depends on resin viscosity, fiber residence time in the bath (path length divided by line speed), tension on the fibers, opening of the strands and sizing compatibility. Gentle heating of the bath lowers viscosity but shortens the resin's working life.
Bath control
- Keep the resin level constant; add fresh resin continuously or in small batches.
- Monitor bath temperature; a rise due to heat from the die or surroundings can cause premature gelation.
- Fillers settle; gentle stirring is needed.
- Resin returning from the die entrance and preformer can be recycled, provided it is filtered and not contaminated with gel.
Preforming
Preformers are a set of guide plates (PTFE, UHMW polyethylene or steel) that bring the wet fibers step by step closer to the final section shape. Their functions:
- Placing each layer (roving, mat, veil) in its exact position in the section
- Gradually folding mat around corners and preventing tearing or wrinkling
- Removing excess resin before the die and reducing back pressure
- Aligning the whole bundle with the die axis
In hollow sections, a mandrel held from upstream (behind the preformer) extends into the die and forms the internal void; the mandrel may itself be heated so that cure also occurs from the inside.
Handbook of Pultrusion Technology
8Die design and manufacture
The die is the heart of the process and the most expensive tooling item. It does three things at once: final shaping, heat transfer for cure, and withstanding pressure and wear.
Material and manufacture
- High-hardness tool steel, precisely machined and polished; the internal surface is usually coated with hard chrome plating so it is smooth and resistant to wear from glass fibers and fillers.
- Dies are usually made in two or more pieces (parting line) so that machining, polishing, cleaning and repair are possible. The parting line should be placed where its effect on appearance matters least.
- Typical die length is about 60 to 150 cm; a longer die allows higher speed but raises friction and cost.
Die geometry
- Tapered or flared entrance (Entrance taper / Radius): to guide the fibers, drain excess resin and prevent the mat from catching.
- Cavity dimensions: resin shrinkage and steel thermal expansion must be allowed for. Because the cured part shrinks on cooling, the cavity is made slightly larger than the final dimensions.
- Corner radii: sharp corners cause resin build-up, gaps and mat tearing; suitable inside and outside radii are essential.
- Uniform wall thickness in section design ensures uniform cure and lower residual stress.
Heating
Heating is usually done with electric platen or cartridge heaters placed in several independent zones along the die, each with its own thermocouple and controller. Hot oil is another option. At the die entrance, water cooling is sometimes used so the resin does not gel before reaching the right place.
Die maintenance
- Clean only with soft tools (brass, wood, plastic); scratches in the chrome are a source of sticking and surface defects.
- Periodic inspection of chrome wear and re-plating before the base steel is reached.
- During long stoppages, keep the line full of cured material or empty and clean the die completely.
Handbook of Pultrusion Technology
9Thermal profile and cure behavior in the die
The book's most important scientific concept is that material passes through three zones along the die, and the positions of these zones are set by temperature and speed:
- Liquid zone: the resin warms and thins (viscosity first drops), air is expelled and the fibers are compacted. Hydraulic resin pressure is high at the entrance.
- Gel zone: the reaction starts and the material becomes rubbery. This is where adhesion to the wall is greatest. With the heat of reaction, the temperature at the part center rises above the die wall (peak exotherm).
- Solid zone: the part has hardened, shrinkage separates it from the wall and cure is completed. The part must reach a sufficient degree of cure before exiting.
Components of pull force
Pull force is the sum of several components: fiber compaction force at the entrance, viscous drag of the liquid resin, adhesive resistance in the gel zone and friction in the solid zone. Continuous monitoring of pull force is the best indicator of process health; a gradual increase usually means deposit build-up in the die or the gel point moving toward the entrance.
Setup rules
- Die temperature for polyester is usually about 120 to 160 °C and higher for epoxy; the entrance zone is set cooler and the middle zones hotter.
- Increasing speed moves the gel point toward the exit; if it moves out of the die, incomplete cure results.
- Too high a temperature or too much initiator pulls the gel toward the entrance and causes sticking and surface sloughing.
- In thick sections, the temperature difference between center and surface is large and the peak exotherm can create internal cracks; solution: more filler, a slower initiator, preheating or lower speed.
Handbook of Pultrusion Technology
10Pulling system, saw and machinery
Types of puller
| Type | Mechanism | Advantages | Limitations |
|---|---|---|---|
| Caterpillar (Caterpillar / Belt) | Two belts or chains with gripping pads that squeeze the part between them and move continuously | Fully continuous, smooth motion; suitable for high speeds and simple sections | Pads must match the section shape; more limited pull force |
| Reciprocating clamp (Reciprocating clamp) | Two clamp units that alternately grip the part, pull and return (hydraulic or electric) | High pull force; suitable for large and complex sections; easy jaw changes | Needs precise synchronization for uninterrupted motion |
| Intermittent (Intermittent) | Pull, stop, pull | Simple and cheap; allows stationary cure in some processes | Stop marks on the part; low speed |
Key machine specifications
- Pull force capacity: from a few tonnes for small rods to several tens of tonnes for wide, thick profiles. The machine should be chosen with a safety margin over the predicted force.
- Speed range: usually from a fraction of a meter to a few meters per minute; typical structural profiles are produced at about 0.3 to 1.5 m/min and thin rods faster.
- Section envelope: the maximum width and height that the clamps and die platform accept.
- Control: constant speed, pull force recording, zone temperatures, length counter and overload alarm.
Cut-off saw
The saw is mounted on a carriage that moves at line speed during the cut (flying saw) so the cut is square and the line doesn't stop. A diamond or abrasive blade is used with water cooling or strong dust extraction; glass and resin dust must be collected.
Plant layout and space
The total line length is usually more than 15 to 20 meters. Enough space must be planned for the roving creel, die access for repair, a cooling zone before the puller and an outfeed table for long products. Local extraction above the bath and die is essential.
Handbook of Pultrusion Technology
11Formulation and fiber layup calculations
Reference formulation example (isophthalic polyester, general profile)
The book expresses formulations in parts per hundred parts of resin (phr). The table below is a typical teaching formulation and a starting point for trials, not a definitive recipe:
| Component | phr | Description |
|---|---|---|
| Isophthalic polyester resin | 100 | Formulation base |
| Low-temperature initiator (peroxydicarbonate) | 0.2–0.5 | Early start of gelation |
| High-temperature initiator (t-butyl perbenzoate) | 0.5–1.0 | Completing cure |
| Internal release agent | 1–2 | Increases with more filler |
| Filler (calcium carbonate or kaolin) | 15–30 | Controlling shrinkage and cost |
| Pigment paste | 2–4 | As required for color |
| UV absorber (for outdoor use) | 0.2–0.5 | Optional |
Mixing sequence
- Resin in a clean container; add the release agent and stir.
- Add filler gradually with a high-speed mixer until fully dispersed and free of lumps.
- Add pigment and other additives.
- Finally, after the mix has cooled, add the initiators with gentle stirring. Never mix initiators directly with each other or with an accelerator.
- Record the viscosity and gel time of each batch for traceability.
Calculating the number of rovings
Example: a 10 mm diameter solid rod (area 78.5 mm²), target fiber volume fraction 60%, E-glass with density 2.54 and 4400 tex roving. Fiber mass per meter = 78.5 × 0.6 × 2.54 ≈ 119.6 g; divided by 4.4 g/m ≈ 27 roving ends. In sections with mat, the mat share (from areal weight × width) is subtracted first and the remainder is filled with roving.
Converting weight percent to volume percent
For example, 70% by weight of glass with density 2.54 in a matrix with density 1.2 (no filler) is roughly equivalent to 52% by volume. Filler raises the matrix density and must be accounted for in the calculation.
Handbook of Pultrusion Technology
12Product design and mechanical properties
Typical properties of glass/polyester profiles compared with metals
| Property | Pultruded profile (longitudinal) | Unidirectional rod | Structural steel | Aluminum 6061-T6 |
|---|---|---|---|---|
| Density (g/cm³) | 1.7–1.9 | 1.9–2.1 | 7.85 | 2.70 |
| Tensile strength (MPa) | 200–300 | 600–1000 | 400–550 | ~310 |
| Tensile modulus (GPa) | 17–28 | 40–48 | 200 | 69 |
| Transverse tensile strength (MPa) | 40–70 | Low | Isotropic | Isotropic |
| Coefficient of thermal expansion (×10⁻⁶/°C) | ~6–9 | ~5–7 | ~12 | ~23 |
| Electrical conductivity | Insulating | Insulating | Conductive | Conductive |
Values are approximate and for general comparison.
Rule of mixtures
With Ef≈72 GPa (E-glass), Em≈3.5 GPa and Vf=0.6, a longitudinal modulus of about 45 GPa is obtained, which agrees with unidirectional rods. In profiles with mat, the share of longitudinal fibers is smaller and the longitudinal modulus lower.
Structural design principles
- Stiffness usually governs, not strength: because of the low modulus, the design criterion is mostly deflection and local buckling of flanges and webs.
- Creep and long-term load: the allowable stress for permanent load must be limited with creep reduction factors.
- Temperature: properties drop as the resin's glass transition temperature is approached.
- Connections: bolts and adhesives are both common; bolted joints need sufficient edge distance and attention to bearing and shear-out. Drilling exposes fibers, and cut edges must be sealed with resin.
- Safety factors higher than for metals (typically 2 to 3 and more) given the brittle failure behavior and the environment.
Section design rules for pultrudability
- Uniform wall thickness; avoid abrupt thickness changes.
- Adequate corner radii; a sharp inside corner is a weak point and collects resin.
- Symmetric layup to prevent warping and bowing.
- Realistic dimensional tolerances; pultrusion tolerances are usually looser than for extruded metal.
Handbook of Pultrusion Technology
13Quality control and testing
The book sees quality control at three levels: incoming material control, in-process control and final product testing. The aim is to identify problems before hundreds of meters of scrap are produced.
1. Incoming material control
- Resin: viscosity, gel time and peak temperature (SPI test), solids content, color.
- Fibers: tex, sizing content (loss on ignition), moisture, package quality.
- Mat and veil: areal weight, binder solubility in styrene, uniformity.
- Filler and initiator: particle size, moisture; production date and storage conditions of initiators.
2. In-process control
- Continuous recording of speed, pull force and die zone temperatures.
- Bath temperature and viscosity; gel time of a batch sample.
- Visual inspection of the surface at exit; dimensional measurements at regular intervals.
- Barcol hardness on the exiting part for a quick assessment of degree of cure (compared with the reference value for a fully cured part).
3. Final product tests (common ASTM standards)
| Property | Standard | Application |
|---|---|---|
| Tensile strength and modulus | ASTM D638 / D3916 (rod) | Longitudinal design properties |
| Flexural strength and modulus | ASTM D790 | Daily quality control; sensitive to cure and adhesion |
| Compressive strength | ASTM D695 | Columns and compression members |
| Interlaminar shear (short beam) | ASTM D2344 | Impregnation quality and fiber/resin adhesion |
| Fiber content (burn-off) | ASTM D2584 | Verifying fiber content |
| Barcol hardness | ASTM D2583 | Degree of cure |
| Density | ASTM D792 | Detecting porosity |
| Water absorption | ASTM D570 | Surface quality and cure |
| Classification of visual defects in pultrusion | ASTM D4385 | Visual acceptance criteria |
| Fire behavior | ASTM E84 / D635 | Flame spread and smoke |
Handbook of Pultrusion Technology
14Process troubleshooting
This is the most practical part of the book for the shop floor. The recommended method: change only one variable at a time, wait for the line to stabilize and record the result.
| Defect | Likely causes | Corrective action |
|---|---|---|
| Surface cracks or microcracks | Severe exotherm, high temperature, low filler, high shrinkage | Lower temperature or fast initiator, more filler, add LPA or veil |
| Surface sloughing and flaking (Sloughing), deposits in the die | Premature gel at the entrance, insufficient release, chrome scratches | Cool the entrance, increase release, polish or re-plate the die |
| Incomplete cure (low Barcol, tackiness, styrene odor) | Low temperature, high speed, insufficient or old initiator | Raise temperature or lower speed, check the initiator |
| Blisters and bubbles | Moisture in fibers or filler, volatiles, incomplete cure, temperature too high | Dry the materials, correct the temperature profile |
| White or dry fibers | Poor impregnation, high viscosity, high speed, unsuitable sizing | Lower viscosity, increase residence time, change roving |
| Fiber prominence (Fiber prominence) | Resin shrinkage, resin-poor surface | Surface veil, LPA, fine filler |
| Twisting and bowing | Asymmetric fiber layout, unequal top and bottom temperatures, residual stress | Make the layup symmetric, equalize die platen temperatures |
| High or fluctuating pull force | Too much fiber, premature gel, low release, deposits | Remove one or two ends, adjust temperature, clean |
| Internal cracks or delamination in thick sections | Temperature difference between center and surface, high peak exotherm | Slower initiator, preheating, lower speed |
| Mat tearing or wrinkling | Soluble mat binder, aggressive preforming, high tension | Mat suited to pultrusion, correct the preformer |
| Color streaks | Poor pigment dispersion, settling | Better mixing, stir the bath |
| Dimensional deviation | Die wear, change in shrinkage, improper fill | Inspect the die, stabilize the formulation |
Handbook of Pultrusion Technology
15Production economics, safety and environment
Cost structure
In pultrusion, raw materials are the largest share of cost (usually more than half the unit cost), followed by machine overhead, die depreciation, labor and scrap. Because the process is continuous, the labor share per meter is small, and line speed and uptime are the main levers for reducing cost.
- Material cost: calculated from the weight per meter and the percentage of each component (fiber, resin, filler, additives); cheap filler lowers cost but affects properties and die wear.
- Start-up: the time to reach acceptable product and initial scrap are a large share for short orders; low volumes must be covered with a higher price.
- Multi-cavity: producing several small profiles at once in one die multiplies productivity.
- Pricing: based on weight or length, but always weighed against the life-cycle cost of the metal competitor.
Safety
- Styrene: its vapor is flammable and has an occupational exposure limit; local extraction above the bath, bath covers and suitable respirators are needed.
- Organic peroxides: strong oxidizers, sensitive to heat and contamination. Store them in a separate cool store, in their original containers and away from accelerators. Mixing peroxide directly with an accelerator can be explosive.
- Fibers and cutting dust: skin and respiratory irritation; gloves, long sleeves, goggles and dust extraction at the saw.
- Mechanical and thermal hazards: the hot die surface, pinch points in the puller and the moving saw require guards, emergency stops and training.
- Fire: resin, solvents and dust are flammable; housekeeping and suitable extinguishing equipment are essential.
Environment
Reducing styrene emissions (covered baths, low-styrene resins, injection impregnation), managing uncured waste resin (full cure before disposal) and reducing cutting waste are concerns raised in the book. The product's environmental advantage is its long life and no need for painting or maintenance.
Handbook of Pultrusion Technology
16Advanced processes and outlook
Radio-frequency preheating (RF Preheating)
In thick sections, heat takes time to reach the center from the die wall. Passing the wet material through an RF field before the die heats the whole volume uniformly, increasing line speed and reducing the center-to-surface temperature difference. The book considers this one of the important tools for increasing productivity in bulky sections. Microwave and induction heating have been proposed along the same lines.
Pulforming (Pulforming)
A variant of the process in which material is shaped after pulling in moving or rotating molds and can have a variable section or curved shape; for example, automotive leaf springs and tool handles. This method partly overcomes the "constant section" limitation of classic pultrusion.
Curved pultrusion (Curved Pultrusion)
Producing profiles with constant curvature using a curved die and a rotating puller; used for arched structural parts and springs.
Pull-winding (Pull-winding)
Combining pultrusion with filament winding: a rotating winding head wraps hoop or helical fiber layers over the longitudinal roving to make tubes with high internal pressure resistance and transverse strength.
Thermoplastic pultrusion
Using a thermoplastic matrix (such as polypropylene, nylon or engineering polymers) with pre-impregnated or powder-coated fibers. Advantages: toughness, weldability, post-formability and recyclability; challenge: very high melt viscosity and difficult impregnation.
Advanced and hybrid fibers
Combining carbon with glass in one section (carbon at the points farthest from the neutral axis for bending stiffness) is an economical way to increase stiffness. Using carbon with epoxy or vinyl ester has expanded for light, stiff applications.
Handbook of Pultrusion Technology
17Conclusions and line start-up checklist
The book's ten golden rules
- Pultrusion is a balance of three variables: die temperature, pull speed and formulation reactivity.
- The gel point must be in the right, stable place in the die; its movement is the root of most defects.
- The product is inherently anisotropic; design transverse properties with mat or fabric.
- Calculate fiber fill, then adjust it experimentally.
- Internal release and chrome surface quality are the keys to low pull force and a sound surface.
- Filler is both a cost-reduction tool and a tool for controlling shrinkage and cracking.
- Multi-stage initiators make fast, complete cure possible without premature gel.
- Record pull force constantly; it is the best early warning.
- In structural design, stiffness and creep usually govern, not strength.
- Profitability depends on uptime and low scrap.
Pre-start-up checklist
- Die clean, inspected and coaxial with the preformer
- Heating zones at set temperature and stable
- Number and path of rovings as per the data sheet
- Mat and veil at the right width and position
- Resin batch with recorded gel time and viscosity
- Low initial speed and gradual increase
- Puller clamp pressure and pads adjusted
- Ventilation, saw extraction and safety equipment active
- First sample: Barcol, dimensions and appearance
- Record all parameters in the shift report
Handbook of Pultrusion Technology
18Glossary
| English term | Meaning | Short explanation |
|---|---|---|
| Pultrusion | Pultrusion | Continuous production of composite profiles by pulling through a heated die |
| FRP | Fiber-reinforced polymer | Resin and fiber composite |
| Roving | Roving | Bundle of parallel continuous strands |
| CSM | Continuous strand mat | Random reinforcement for transverse properties |
| Surfacing veil | Surface veil | Thin layer for a resin-rich surface |
| Creel | Roving creel | Holder for fiber packages |
| Preformer | Preformer | Guides wet fibers into the section shape |
| Mandrel | Mandrel | Internal core for hollow sections |
| Gel point | Gel point | Transition of liquid resin to a rubbery state |
| Peak exotherm | Peak exotherm | Maximum temperature from the cure reaction |
| Initiator / Catalyst | Initiator / catalyst | Peroxide that starts cure |
| Internal mold release | Internal release agent | Anti-stick additive in the formulation |
| Filler | Filler | Mineral powder for cost and shrinkage |
| LPA | Low-profile additive | Compensates cure shrinkage |
| Sizing | Sizing | Fiber surface coating for compatibility with resin |
| Tex / Yield | Tex / yield | Mass per length or length per mass of fiber |
| phr | Parts per hundred parts of resin | Formulation unit |
| Barcol hardness | Barcol hardness | Quick indicator of degree of cure |
| Sloughing | Surface sloughing | Defect caused by sticking to the die |
| Fiber prominence | Fiber prominence | Fibers showing at the surface |
| Puller | Puller | System that applies pull force |
| Rule of mixtures | Rule of mixtures | Estimating properties from the constituents' shares |
| Pulforming | Pulforming | Pultrusion variant with variable or curved section |