Structural Design of Polymer Composites — EUROCOMP Code
Structural Design of Polymer Composites

Structural Design of Polymer Composites — EUROCOMP Design Code and Handbook

Structural Design of Polymer Composites: A Comprehensive Summary of the EUROCOMP Design Code and Handbook

A limit-state design code for FRP structures: basis of design, partial material factors, characteristic values, laminates, design of members and plates, buckling, deflection and creep, durability, bolted and bonded joints, manufacture and quality control

Editor of the original book: John L. Clarke
Publisher: E & FN Spon — the outcome of the joint European EUROCOMP project
Prepared for: NABAK Composite

About this book

EUROCOMP was the first comprehensive European attempt to draft a structural design code for fiber-reinforced polymer (FRP) composites with the same structure as the Eurocodes for steel and concrete. The book has two main parts: the design code (principles and application rules) and the handbook (explanations, scientific background, analysis methods and design examples). Although many years have passed since its publication, its philosophy became the basis of later European codes and FRP profile design guides, and it is still a reference for designing pultruded structures.

How to use this summary

  • Orange "Key point" boxes give the most important design rule of each chapter.
  • Gold "Note" boxes give a practical interpretation for FRP profile manufacturers and designers, or point to later codes.
  • Numerical values of factors and limits in this summary are approximate and meant to show scale; for real design, use the original tables of the code or the current national standard.
NABAK CompositePage 1 of 20
Structural Design of Polymer Composites — EUROCOMP Code
Structural Design of Polymer Composites

Table of Contents

  1. 1Background and structure of the EUROCOMP code
  2. 2Basis of design: limit states, actions and combinations
  3. 3Partial material factors (γm)
  4. 4Materials and characteristic values
  5. 5Laminate properties and analysis
  6. 6Ultimate limit state: tension, compression, bending and shear
  7. 7Stability: buckling of members and components
  8. 8Plates and sandwich panels
  9. 9Serviceability limit state: deflection, vibration and creep
  10. 10Durability, environment and fire
  11. 11Connections: selection and general principles
  12. 12Bolted connections
  13. 13Bonded and combined connections
  14. 14Manufacture, quality control and testing
  15. 15Design procedure example for an FRP profile beam
  16. 16The EUROCOMP legacy and later codes
  17. 17Conclusions and frequently asked questions
  18. 18Glossary of FRP structural design terms
The book's main message in one sentenceAn FRP structure can be designed with the same limit-state logic as steel and concrete, provided three fundamental differences are taken into account: anisotropy and transverse weakness, the strong dependence of properties on the manufacturing process, and the effect of time and environment on behavior; these three are built into the code's partial factors and design rules.
NABAK CompositePage 2 of 20
Structural Design of Polymer Composites — EUROCOMP Code
Structural Design of Polymer Composites

1Background and structure of the EUROCOMP code

In the 1990s, structural use of FRP composites in buildings, bridges, industry and marine applications was growing, but the lack of a design code was the main barrier to acceptance by engineers and clients. The EUROCOMP project, with industrial and research organizations from several European countries, drafted a code in the style of the Eurocodes.

Scope

  • Building and civil engineering structures and structural components made of glass-fiber polymer composites (and, to a limited extent, carbon and aramid).
  • Thermoset matrices: polyester, vinyl ester, epoxy and phenolic.
  • Manufacturing methods: pultrusion, hand lay-up and spray-up, RTM and infusion, filament winding, prepreg.
  • Linear members (profiles), plates, sandwich panels and connections.

Structure of the book

PartContent
Design codeChapters on general matters, basis of design, materials, ultimate limit state, serviceability limit state, connections, manufacture, quality control and testing
HandbookExplanation and background of each code clause, analysis methods, material data, buckling and connection formulas, design examples
Appendices and examplesStep-by-step design of members and connections

Principles and application rules

As in the Eurocodes, code clauses are of two kinds: principles (P), which are mandatory and have no alternative, and application rules, which are accepted methods of satisfying the principles; equivalent alternative methods may be used if they are proven.

General approach

Limit-state design with partial load factors according to the Eurocode on actions, and composite-specific partial material factors that account for the source of the data, the manufacturing process, and environmental and time effects. "Design assisted by testing" is also accepted as a valid route.

Key pointEUROCOMP does not force the engineer to know the material exactly; but the less is known about the material (theoretical data instead of tests, a less controlled process), the larger the partial factor and the heavier the design. "Knowledge reduces weight."
NABAK CompositePage 3 of 20
Structural Design of Polymer Composites — EUROCOMP Code
Structural Design of Polymer Composites

2Basis of design: limit states, actions and combinations

Fundamental requirements

With appropriate reliability and economy, the structure must withstand the likely actions and effects over its design life, remain fit for its intended use and be adequately durable; it must also not suffer damage disproportionate to accidents (impact, fire, explosion).

Limit states

Limit stateExamples in FRP structures
Ultimate (ULS)Material rupture, local and global buckling, connection failure, instability of the whole structure, creep rupture
Serviceability (SLS)Excessive deflection, annoying vibration, matrix cracking and visible damage, long-term deformation due to creep

Design situations

Persistent (normal use), transient (transport and erection), accidental (impact, fire). For each situation the appropriate load combination and material factors are chosen; for example, during erection the load is short-term and the load-duration factor is smaller.

Partial load factors and combinations

E_d = Σ γ_G·G_k + γ_Q,1·Q_k,1 + Σ γ_Q,i·ψ₀,i·Q_k,i    (ULS, fundamental combination)

Load factors follow the Eurocode on actions (for example about 1.35 and 1.5 for dead and imposed loads when unfavorable). For SLS, characteristic, frequent and quasi-permanent combinations with factors of 1.0 and ψ factors are used. The quasi-permanent combination is especially important for calculating creep and long-term deflection.

Design condition

E_d ≤ R_d     R_d = R(X_k / γ_m)

The design effect of actions must not exceed the design resistance; the design resistance is calculated from the characteristic property values divided by the partial material factor.

Design assisted by testing

The code allows the capacity of a member or connection to be determined by testing real specimens; the results are converted to characteristic values with statistical methods and reduced to design resistance with appropriate factors. This route is very useful for manufacturers' profiles and connections.

Key pointThe structure of the load combinations is the same as in the Eurocode; the main difference for FRP structures lies on the "resistance" side and in the importance of long-term (quasi-permanent) combinations for creep.
NABAK CompositePage 4 of 20
Structural Design of Polymer Composites — EUROCOMP Code
Structural Design of Polymer Composites

3Partial material factors (γm)

The heart of the EUROCOMP code and its most important difference from metal codes: the partial material factor is built from three parts, each covering one source of uncertainty.

γ_m = γ_m,1 × γ_m,2 × γ_m,3     X_d = X_k / γ_m
FactorSource of uncertaintyTrend of value
γ_m,1How material properties are determinedLowest for properties obtained by testing the same material and process; higher for properties calculated by theory (micromechanics, laminate theory); highest for generic, indirect data
γ_m,2Manufacturing method and degree of cureLowest for controlled, automated processes (pultrusion, prepreg, filament winding, RTM) with full post-cure; higher for hand lay-up and spray-up without post-cure
γ_m,3Service environment and load durationLower for short-term loads and service temperatures well below the resin's heat deflection temperature (HDT); much higher for long-term loads and service temperatures near the HDT

Interpretive notes

  • γ_m,3 is the largest factor: for long-term loads, creep and creep rupture noticeably increase the factor; for short-term loads it is close to one.
  • Temperature dependence: the smaller the gap between service temperature and the resin's HDT, the larger γ_m,3; this means choosing a resin with a higher HDT directly increases design capacity.
  • Serviceability limit state: for stiffness at SLS, smaller factors are used (and, for long-term deflection, a creep-reduced modulus).
  • The code sets a minimum for the overall factor at ULS so that a combination of small factors does not reduce safety too far.

Comparison with steel

The material factor for steel in the Eurocode is about 1.0 to 1.25; the overall FRP factor for long-term loads can be several times higher. This difference reflects the greater scatter of data, the sensitivity to the process, and the time- and environment-dependent behavior of composites.

Note for FRP profile manufacturersThree actions by the manufacturer directly reduce the factors and increase the design capacity of the product: providing properties tested on the actual profile (γ_m,1), guaranteeing full cure and quality control (γ_m,2), and using a resin with a high HDT (γ_m,3).
Key pointγ_m tells the engineer "how much to trust the material"; valid test data, a controlled process and a suitable resin raise that trust and lower the weight of the structure.
NABAK CompositePage 5 of 20
Structural Design of Polymer Composites — EUROCOMP Code
Structural Design of Polymer Composites

4Materials and characteristic values

Constituents

  • Fibers: E-glass (main), S-glass, carbon and aramid; in the form of roving, mat, woven and stitched fabrics.
  • Resins: ortho and iso polyester, vinyl ester, epoxy, phenolic; with a specified heat deflection temperature (HDT) and glass transition temperature.
  • Sandwich cores: polymer foams, balsa wood, honeycomb.
  • Adhesives: epoxy, acrylic, polyurethane.

Characteristic values

X_k = X_mean − k_n·s    (5% fractile, with k_n depending on number of tests and confidence)

The characteristic strength is the 5th percentile of the statistical distribution at a specified confidence level; the factor k_n increases as the number of tests decreases, so more tests lead to a higher characteristic value. For stiffness, the mean value is usually used.

Methods for determining properties

  1. Testing the actual material: specimens cut from the product or production laminate (most reliable; lower γ_m,1).
  2. Calculation from constituent properties: micromechanics (rule of mixtures) and laminate theory; requires fiber, resin and volume-fraction data.
  3. Generic data: typical values given in the handbook for preliminary design (higher γ_m,1).

Properties required for design

GroupProperties
StiffnessLongitudinal and transverse tensile and compressive moduli, in-plane and interlaminar shear moduli, Poisson's ratio
StrengthTensile, compressive, in-plane and interlaminar shear in the principal directions; bearing
Time-dependentCreep coefficients, creep-rupture strength, fatigue
PhysicalDensity, coefficient of thermal expansion, HDT and Tg, water absorption
Key pointIn FRP, the "material" is not independent of the "product"; the properties of a laminate with the same fibers and resin change with the process, volume fraction and layup. Characteristic values must apply to the same process and layup used in the structure.
NABAK CompositePage 6 of 20
Structural Design of Polymer Composites — EUROCOMP Code
Structural Design of Polymer Composites

5Laminate properties and analysis

The EUROCOMP handbook provides tools to calculate laminate properties from the plies so the designer can estimate stiffness and strength for any layup.

From ply to laminate

  1. Properties of each ply from the constituents (rule of mixtures for the longitudinal direction and semi-empirical relations for the transverse and shear directions) or from tests.
  2. Ply stiffness matrix in material axes and its transformation to structural axes based on the ply angle.
  3. Forming the A, B and D matrices with classical laminate theory.
  4. Calculating the effective engineering constants of the laminate (in-plane and flexural moduli and Poisson's ratios).
{N; M} = [[A, B], [B, D]]·{ε⁰; κ}    E_x = 1/(h·a₁₁), E_x,flex = 12/(h³·d₁₁)

Discontinuous plies

For random mats (CSM and CFM), common in hand lay-up and pultrusion, approximately in-plane isotropic behavior is assumed and properties are estimated with empirical relations based on fiber weight content. The handbook gives simple relations for the modulus and strength of mats and fabrics in terms of fiber content.

Laminate strength

  • The stresses in each ply from the laminate analysis are transformed to material axes and compared with a failure criterion (maximum stress or strain, and quadratic interaction criteria).
  • The code's conservative approach: first-ply failure is the ultimate limit state design criterion, especially when matrix cracking would lead to moisture ingress and reduced durability.
  • As a simple alternative, design based on an allowable strain for the laminate.

Layup considerations

Symmetric and balanced laminates to eliminate coupling and warping; a minimum number of plies in different directions for secondary loads; avoiding abrupt thickness changes; and attention to interlaminar stresses at edges and holes.

Note for FRP profilesFor pultruded profiles, the code prefers that the properties of each wall (flange, web) be taken from tests on the profile or from the manufacturer's certified data, because the roving and mat layup in the walls is not always exactly known.
Key pointLaminate theory is a tool for designing the layup, but its accuracy depends on the ply properties; for final design, calibrating with tests on the actual laminate reduces γ_m,1.
NABAK CompositePage 7 of 20
Structural Design of Polymer Composites — EUROCOMP Code
Structural Design of Polymer Composites

6Ultimate limit state: tension, compression, bending and shear

For linear members (especially pultruded I, H, channel, angle, box and tube profiles), the code provides design rules similar to the Eurocode for steel, with the changes needed for anisotropy and transverse weakness.

ActionCheckFRP-specific notes
Axial tensionN_Ed ≤ A·f_t,dReduced cross-section at holes and stress concentration; in FRP, stress concentrations are not redistributed by yielding
Axial compressionN_Ed ≤ A·f_c,d and buckling checkCompressive strength lower than tensile; buckling often governs
FlexureM_Ed ≤ W·f_d and check of local and lateral-torsional bucklingNo plastic capacity; fully elastic design
ShearV_Ed ≤ A_w·f_v,dLow in-plane shear strength of the web; shear at the web–flange junction
TorsionTorsional stiffness and strengthOpen sections have very low torsional stiffness; closed sections preferred
Combined actionsLinear interaction relationsConservative; includes second-order effects in combined compression and bending

Important principles

  • Linear elastic analysis: because FRP does not yield, plastic moment redistribution or plastic design is not allowed.
  • Shear deformation: must be included when calculating internal forces in statically indeterminate structures and in deflection, because of the low shear modulus.
  • Stress concentration: local and transverse stresses must be checked at inner corners of profiles, holes and changes of section.
  • Second-order effects: because of the low modulus, deformations are larger and P-Δ effects are important in compression members and frames.
Key pointIn FRP design there is no "ductility"; no plastic capacity or force redistribution should be assumed. The safety margin comes from the partial factors and careful detailing, not from material behavior after yielding.
NABAK CompositePage 8 of 20
Structural Design of Polymer Composites — EUROCOMP Code
Structural Design of Polymer Composites

7Stability: buckling of members and components

Because of the high strength-to-stiffness ratio and thin walls, stability often governs the design of FRP members. The handbook gives analytical and semi-empirical relations for the various buckling modes.

Global column buckling

N_cr = π²·E·I / (β·L)²     with shear: 1/N_cr,eff = 1/N_E + 1/(k·G·A)

Shear reduces the buckling load. For columns of intermediate slenderness, the interaction between compressive strength and buckling is captured with design curves (similar to steel column curves but with composite parameters) and an initial geometric imperfection.

Local buckling

Profile walls (flanges and web) are orthotropic plates with boundary conditions that depend on their connection to adjacent walls:

σ_cr,local = k·π²·√(D₁₁·D₂₂) / (t·b²)    (orthotropic plate; k depends on edge restraint and stiffness ratios)
  • Outstanding flanges (one free edge): lowest capacity; governing in I-beams and channels.
  • Internal flanges and webs (two connected edges): higher capacity; box sections.
  • Web under shear and bending: web shear buckling in deep beams.

Lateral-torsional buckling

Open beams without lateral restraint suffer lateral-torsional buckling because of their low torsional and lateral stiffness. The critical moment is calculated with classical relations and the effective FRP stiffnesses (E and G), and is controlled with adequate lateral restraint.

Web crushing and concentrated loads

At supports and under concentrated loads, the web is under transverse compression (perpendicular to the longitudinal fibers), which is weak in FRP; web stiffeners or load-spreading plates are needed.

Mode interaction

Interaction between local and global buckling, and between buckling and strength, makes the capacity lower than for any single mode; the code recommends using reduction factors or testing.

Key pointThe width-to-thickness ratio of the walls is the key to FRP profile design; a thicker, narrower wall delays local buckling and is usually more economical than improving the material.
NABAK CompositePage 9 of 20
Structural Design of Polymer Composites — EUROCOMP Code
Structural Design of Polymer Composites

8Plates and sandwich panels

Laminated plates

Plates (floors, walls, tank shells, decks) are analyzed with orthotropic plate theory. The handbook gives tables and relations for deflection, moment and buckling load of rectangular plates with common boundary conditions under uniform and concentrated loads. For thick plates, transverse shear deformation is included.

Sandwich panels

D ≈ E_f·t_f·d²/2    S ≈ G_c·d    δ = δ_bending + δ_shear

The composite skins carry bending through membrane stresses and the core carries shear. The code requires the following checks:

CheckDescription
Skin strengthTensile and compressive skin stress against the design strength of the laminate
Core shearCore shear stress against the design shear strength of the core
Face wrinklingLocal buckling (wrinkling) of the compression skin on the core foundation
Global panel bucklingTaking the core shear stiffness into account
Local indentationUnder concentrated loads and at supports; inserts or reinforcement needed
Skin–core bondNormal tension and shear at the interface
DeflectionIncludes the core shear contribution, which can dominate
Core creepPolymer foam cores have significant creep

Practical considerations

Inserts for connections, edge sealing to prevent water from entering the core, and the thermal and fire behavior of polymer cores.

Key pointIn a sandwich panel, the core is as much a "structural material" as the skins; core shear, creep and bond often govern the design and must be checked as carefully as the skins.
NABAK CompositePage 10 of 20
Structural Design of Polymer Composites — EUROCOMP Code
Structural Design of Polymer Composites

9Serviceability limit state: deflection, vibration and creep

Because of the relatively low modulus of glass composites, the serviceability limit state often governs the dimensions of FRP members. The code covers this part in more detail than the metal Eurocodes.

Deflection

  • Total deflection = bending deflection + shear deflection + creep deflection.
  • Deflection limits are set according to the application (for example span/250 to span/500) and the member type (floor beams, roofs, members carrying sensitive equipment).
  • For short-span pultruded profiles and sandwich panels, shear deflection can be a large part of the total deflection.

Creep

E(t) = E₀ / (1 + φ(t))    or   ε(t) = ε₀ + m·tⁿ

Long-term deflection under the quasi-permanent load combination is calculated with a creep-reduced modulus (creep coefficient φ). Creep coefficients depend on direction (lower longitudinally, higher in shear and transversely), resin, stress level, temperature and humidity. The code also sets a long-term stress limit to prevent creep rupture (which is accounted for in γ_m,3).

Vibration

Lightweight FRP structures (footbridges, floors) have low natural frequencies and low mass and are sensitive to vibration from pedestrians and wind. Checking the natural frequency (away from the human pacing range) and the response acceleration is necessary; FRP's better damping compared with steel helps a little.

Cracking and damage

In liquid-retaining applications (tanks, pipes) or in corrosive environments, matrix cracking is itself a limit state; working strain is limited so that microcracks do not form.

Thermal effects

Strains and stresses caused by temperature change and by differential expansion with other components (steel, concrete) are checked at SLS.

Key pointIn FRP design, check SLS first: short-term deflection including shear, long-term deflection including creep, and vibration. Then check ULS; this order usually reaches the right dimensions faster.
NABAK CompositePage 11 of 20
Structural Design of Polymer Composites — EUROCOMP Code
Structural Design of Polymer Composites

10Durability, environment and fire

Environmental factors

FactorEffectDesign solution
TemperatureReduced stiffness and strength, increased creep as the HDT is approachedChoose a resin with sufficient HDT; appropriate γ_m,3
Moisture and waterDegraded matrix and interface properties; osmotic blisteringSuitable resin and fibers, resin-rich layer, full cure
ChemicalsAttack on resin and glass fibers (stress corrosion)Vinyl ester, surface veil, manufacturer's chemical resistance tables
UV and weatheringSurface degradation, fiber bloomingGelcoat, veil, UV absorber, paint
Freeze–thaw cyclesCrack growth in the presence of waterCrack control and sealing
Cyclic loadingFatigue, especially at connectionsStress-range limits; appropriate detailing

The code sets general durability principles and refers to material data and service experience. Design life and environmental conditions must be defined from the start and taken into account when choosing materials and factors.

Fire

  • Polymer resins are combustible; reaction to fire (ignition, flame spread, smoke) and fire resistance (retention of load-bearing capacity) must be checked according to national regulations.
  • Structural properties drop quickly as the resin's Tg is approached; load-bearing members in fire need protection (insulation, coatings) or design for the accidental situation.
  • Phenolic resins and flame-retardant additives improve fire behavior; the effect of additives on mechanical properties must be reflected in the characteristic values.

Inspection and maintenance

The code emphasizes a periodic inspection program (cracks, discoloration, loosening of connections, impact damage) and the possibility of repair.

Key pointFRP durability is not excellent "by default"; it depends on the right choice of resin, full cure, surface protection and proper detailing. The designer must define the environment precisely and the manufacturer must guarantee material compatibility.
NABAK CompositePage 12 of 20
Structural Design of Polymer Composites — EUROCOMP Code
Structural Design of Polymer Composites

11Connections: selection and general principles

The connections section is one of the most detailed and valuable parts of EUROCOMP, because connections are the known weak point of FRP structures and before it there was almost no comprehensive design guidance for them.

Types of connection

TypeAdvantagesDrawbacks
Mechanical (bolts, rivets, self-tapping screws)Simple to install, inspectable and demountable, predictable behavior, tolerant of construction errorsStress concentration at holes, cut fibers, extra weight
BondedBetter load distribution, no holes, sealing, high stiffnessSensitive to surface preparation and workmanship; difficult to inspect; sensitive to environment
Combined (adhesive + bolts)A second load path for safety; holding parts in place during cureComplexity; load carried mainly by the adhesive until damage occurs

General principles of connection design

  • Clear load path: the connection must transfer load without creating large secondary stresses (especially transverse tension and peel).
  • Load along the fibers: design so that load is transferred mainly by in-plane shear or by tension and compression along the fibers.
  • Avoid eccentricity: in single-lap connections, secondary bending reduces capacity.
  • Connection capacity versus member: the connection must either be stronger than the member or have a progressive, predictable failure mode.
  • Environmental conditions: the effect of moisture and temperature on the adhesive, and relaxation of bolt preload.
  • Fabrication and inspection: the connection must be feasible and checkable with shop or site methods.

Selecting the type of connection

The code gives selection criteria: type and size of load (static or cyclic), need for disassembly, member thickness (bonded joints are more effective for thin members, bolted for thick ones), construction conditions (shop or site), environment, and inspection requirements.

Key pointIn an FRP structure, connection design must start together with member design; profile dimensions are often set not by bending but by the need for wall thickness and sufficient spacing for connections.
NABAK CompositePage 13 of 20
Structural Design of Polymer Composites — EUROCOMP Code
Structural Design of Polymer Composites

12Bolted connections

Failure modes

ModeDescriptionMain factor
BearingCrushing of the hole wall under the boltBearing strength; lateral pressure of the washer
Net-section tensionRupture at the section reduced by the holeWidth and edge distance; stress concentration
Shear-outA block pulled out of the end of the memberEnd distance; shear strength
CleavageLongitudinal crack from the hole toward the endTransverse strength; non-longitudinal plies
Bolt pull-through and bolt failureTension along the bolt axis or bolt shearMember thickness, washer size, bolt material

Geometric rules

The code sets minimum distances in terms of bolt diameter (d): end distance, edge distance and bolt spacing. Commonly recommended distances are several times the diameter (end distance usually at least about 3 diameters and bolt spacing about 4 diameters or more); the aim is to make bearing, which fails more progressively, the governing mode. Take exact values from the code tables.

Capacity calculation

  • For each failure mode, a capacity relation is given in terms of the laminate's characteristic strengths (bearing, tensile, shear) and geometry; the connection capacity is the minimum of these values.
  • For tension on the net section, a stress concentration factor that depends on the width-to-diameter ratio and laminate anisotropy is included.
  • In multi-bolt connections, the unequal load distribution among bolts (the first row carries the largest share) is taken into account with spring-stiffness analysis or reduction factors; because FRP lacks ductility, it does not equalize load among the bolts.
  • The direction of load relative to the fibers (longitudinal, transverse or oblique) affects capacity.

Construction details

Small hole clearance, large stiff washers, controlled tightening torque (allowing for relaxation over time), stainless steel bolts, damage-free drilling (proper tools and backing) and sealing of hole edges.

Key pointDesign FRP bolted connections for bearing, not for shear-out or cleavage; adequate distances, transverse plies in the wall and suitable washers ensure this.
NABAK CompositePage 14 of 20
Structural Design of Polymer Composites — EUROCOMP Code
Structural Design of Polymer Composites

13Bonded and combined connections

Common geometries

Single and double lap, single and double strap, stepped, scarf, T and corner joints, and tubular joints. The more symmetric the geometry and the more gradual the load transfer, the lower the stress concentration.

Stress distribution

  • Adhesive shear: in a lap joint it peaks at both ends and is low in the middle (Volkersen analysis); increasing overlap length beyond a certain point adds little capacity.
  • Peel stress: occurs at the ends of the overlap in single-lap joints because of eccentricity (Goland–Reissner analysis); it is the most dangerous stress, since FRP and adhesives are weak in through-thickness tension.
  • Failure in the laminate: failure often occurs not in the adhesive but in the surface ply of the composite (interlaminar separation).

Design method

The code allows simple methods (average shear stress with reduction factors) and more accurate methods (elastic stress analysis or finite element analysis with a combined shear–peel criterion). Partial factors for the adhesive account for workmanship and environmental effects.

Ways to reduce peel

Double instead of single lap joints, tapering the end of the overlap, an adhesive fillet at the ends, scarf and stepped joints, and adhesives with higher failure strain.

Surface preparation and application

  • Removing release agent from profile surfaces by sanding and solvent cleaning, or a peel ply during production.
  • Control of adhesive thickness, ambient cure temperature and humidity, and adhesive open time.
  • Control tests on specimens made at the same time.

Hybrid connections

Alongside the adhesive, bolts act as a secondary load path and as safety against sudden adhesive failure; but because the adhesive is stiffer, the bolts carry little load until the adhesive is damaged. The code recommends designing on the basis of either load path on its own.

Key pointDesign bonded joints for shear and eliminate peel through geometry; their success depends more on surface preparation and quality control of the work than on calculation.
NABAK CompositePage 15 of 20
Structural Design of Polymer Composites — EUROCOMP Code
Structural Design of Polymer Composites

14Manufacture, quality control and testing

Manufacture

The code treats manufacturing requirements as part of design, because material properties are formed during manufacture:

  • Process documentation: materials, layup, fiber fraction, cure and post-cure conditions.
  • Workshop conditions: temperature, humidity, cleanliness and storage of materials (especially resins, adhesives and fibers).
  • Tolerances: dimensions, straightness, twist and fiber misalignment; their effect on buckling and connections.
  • Secondary operations: cutting, drilling, bonding and edge sealing.
  • Transport and erection: preventing impact and local loads during erection.

Quality control

StageChecks
Incoming materialsSupplier certificates, acceptance tests for resin, fibers and adhesive
During manufactureRecording process parameters, visual inspection, checking thickness and layup
Finished productBarcol hardness (degree of cure), fiber content (burn-off), dimensions, visual defects, mechanical tests on specimens
JointsAdhesive witness specimens, checking bolt torque
Non-destructive inspectionTap testing, ultrasonics for delamination and voids

The code assigns different γ_m,2 factors to different levels of quality control; a documented quality management system (such as ISO 9001) is assumed.

Test methods

The testing section gives methods for determining material properties (tension, compression, bending, in-plane and interlaminar shear, bearing, creep) with references to ISO, EN and ASTM standards, plus special methods for profiles and connections. It also defines the statistical method for converting test results into characteristic values.

Load testing

For design assisted by testing or innovative structures, load testing of a full-size specimen or the complete structure is recommended to confirm capacity and behavior.

Key pointIn an FRP structure, quality control is "part of the safety factor"; documented, tested quality reduces the partial factor and increases the client's confidence.
NABAK CompositePage 16 of 20
Structural Design of Polymer Composites — EUROCOMP Code
Structural Design of Polymer Composites

15Design procedure example for an FRP profile beam

The EUROCOMP handbook contains many design examples. The general procedure for designing a simply supported pultruded I-beam under uniform load can be summarized as follows:

Step 1: Data

  • Characteristic loads (dead and imposed) and their duration; span; lateral restraint conditions.
  • Environment: service temperature, humidity, chemicals; design life.
  • Characteristic properties of the profile from the manufacturer (E and G moduli; longitudinal, shear and transverse strengths).

Step 2: Partial factors

Determine γ_m,1 (properties tested on the profile), γ_m,2 (pultrusion with full cure) and γ_m,3 separately for short-term and long-term loads; load factors for the ULS and SLS combinations.

Step 3: Serviceability limit state

δ = 5qL⁴/(384·E·I) + qL²/(8·G·A_w) ≤ L/limit    δ_long-term with E(t), G(t)

Short-term deflection under the characteristic combination and long-term deflection under the quasi-permanent combination with creep-reduced moduli; natural frequency check if needed. This step often determines the profile size.

Step 4: Ultimate limit state

  1. Bending stress in the flanges ≤ longitudinal design strength.
  2. Web shear stress ≤ design shear strength.
  3. Local buckling of the compression flange (orthotropic plate with a free edge).
  4. Lateral-torsional buckling (with the spacing of restraints).
  5. Web crushing at supports; stiffeners if needed.

Step 5: Connections

Design the support connection (angles bolted to the web); check bearing, shear-out and cleavage of the web; check distances.

Step 6: Durability and detailing

Sealing cut edges, UV protection, stainless bolts, preventing water accumulation, and an inspection program.

NoteFRP profile manufacturers can greatly simplify design for their customers by providing "capacity tables" (maximum allowable load versus span for each profile, accounting for deflection, buckling and strength); this approach is common in the catalogs of leading manufacturers.
Key pointThe logical order for designing an FRP beam: deflection (with shear and creep) → buckling modes → strength → connections → durability; all must be checked, but the first two usually set the dimensions.
NABAK CompositePage 17 of 20
Structural Design of Polymer Composites — EUROCOMP Code
Structural Design of Polymer Composites

16The EUROCOMP legacy and later codes

Although EUROCOMP never became an official Eurocode, it was used as an authoritative reference in Europe and beyond and became the conceptual basis of many later guides and codes.

Key achievements

  • Proving that FRP design can be carried out within a limit-state framework consistent with the Eurocodes.
  • The concept of a multi-part partial factor (data source, process, environment and load duration).
  • Systematic design rules for bolted and bonded connections.
  • Emphasis on SLS, creep and durability as an integral part of FRP design.
  • Formal standing for "design assisted by testing".

Later codes and guides

DocumentDescription
EN 13706Specifications for pultruded profiles with grades E23 and E17
CNR-DT 205 (Italy)Guide for the design of structures made of pultruded FRP profiles
CEN/TS 19101European technical specification for the design of FRP structures; a step toward a composites Eurocode
ASCE (USA)Standard for limit-state design of pultruded FRP structures
Guides for FRP bars and strengtheningFor FRP-reinforced concrete and strengthening (such as ACI and fib guides)

These documents continue the same partial-factor philosophy with more data and more up-to-date methods (especially for local buckling and connections). For today's projects, the current national code and the latest editions of these documents must govern.

Key pointUnderstanding EUROCOMP is the key to understanding the new FRP codes; its structure, concepts and even many of its formulas are preserved in later documents.
NABAK CompositePage 18 of 20
Structural Design of Polymer Composites — EUROCOMP Code
Structural Design of Polymer Composites

17Conclusions and frequently asked questions

Ten golden rules of EUROCOMP

  1. Limit-state design with Eurocode load factors and FRP-specific material factors.
  2. γ_m = γ_m,1 × γ_m,2 × γ_m,3; it accounts for material knowledge, process quality, and environment and time.
  3. Characteristic values from statistical testing of material from the same process; more tests, better values.
  4. Linear elastic analysis; no plastic capacity or redistribution.
  5. Include shear deformation in deflection and analysis.
  6. Local buckling, lateral-torsional buckling and web crushing often govern.
  7. SLS (deflection, creep, vibration) usually determines the dimensions.
  8. Durability is ensured by resin selection, full cure and surface protection.
  9. Design bolted connections for bearing and bonded connections for shear; eliminate peel.
  10. Manufacturing quality control is part of the safety factor.

Frequently asked questions

What is EUROCOMP? A structural design code and handbook for polymer composites, prepared in the 1990s in a joint European project, that presents limit-state design of FRP structures in a structure similar to the Eurocodes.

How is the partial material factor determined? As the product of three factors for the source of property data, the manufacturing method and cure, and the environmental conditions and load duration; the design value equals the characteristic value divided by this factor.

Why is SLS important in FRP design? Because the elastic modulus of glass composites is relatively low, and deflection, vibration and creep often govern before strength.

Can EUROCOMP still be used today? Its philosophy and methods remain valid and form the basis of new codes, but for new projects the current code and the latest documents (such as CEN/TS 19101) must govern.

NABAK CompositePage 19 of 20
Structural Design of Polymer Composites — EUROCOMP Code
Structural Design of Polymer Composites

18Glossary of FRP structural design terms

English termMeaningShort explanation
Limit state designLimit-state designDesign philosophy
ULS / SLSUltimate / serviceability limit stateSafety / serviceability
Principles / Application rulesPrinciples / application rulesStructure of code clauses
Partial safety factorPartial safety factorLoad and material
γm,1 / γm,2 / γm,3Factors for data source / process / environment and load durationComponents of the material factor
Characteristic valueCharacteristic valueStatistical 5th percentile
Design valueDesign valueCharacteristic value divided by γm
Quasi-permanent combinationQuasi-permanent combinationFor creep and long-term deflection
Heat deflection temperature (HDT)Heat deflection temperatureTemperature criterion for the resin
Creep coefficientCreep coefficientReduction of modulus over time
Creep ruptureCreep ruptureFailure under sustained load
First ply failureFirst-ply failureConservative laminate criterion
Local buckling / LTBLocal / lateral-torsional bucklingInstability
Web cripplingWeb cripplingConcentrated load
Face wrinklingFace wrinklingSandwich
Bearing / Net-tension / Shear-out / CleavageBearing / net tension / shear-out / cleavageBolted connection
Peel stressPeel stressBonded connection
Single / Double lap jointSingle / double lapJoint geometry
Hybrid (bonded-bolted) jointCombined connectionAdhesive + bolts
Design assisted by testingDesign assisted by testingAlternative load path
Load-span tablesLoad–span tablesProfile design tool
CEN/TS 19101European technical specification for FRPNew code

Related keywords: FRP structural design, composite design code, EUROCOMP, partial material factor, limit state, FRP profile design, bolted and bonded connections, buckling, creep, sandwich panel, composite structure, NABAK Composite.

NABAK CompositePage 20 of 20